Next Article in Journal
Electrospun Alginate Nanofibers Toward Various Applications: A Review
Next Article in Special Issue
Dual-Responsive Nanotubes Assembled by Amphiphilic Dendrimers: Controlled Release and Crosslinking
Previous Article in Journal
Discrete Element Method Modelling of the Diametral Compression of Starch Agglomerates
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Enhanced Microwave Absorption and Electromagnetic Properties of Si-Modified rGO@Fe3O4/PVDF-co-HFP Composites

State Key Lab for Manufacturing Systems Engineering, School of Mechanical Engineering, Xi’an Jiaotong University, Xi’an 710054, China
*
Author to whom correspondence should be addressed.
Materials 2020, 13(4), 933; https://doi.org/10.3390/ma13040933
Submission received: 6 January 2020 / Revised: 6 February 2020 / Accepted: 9 February 2020 / Published: 20 February 2020
(This article belongs to the Special Issue Synthesis and Applications of Nanoparticles)

Abstract

:
Graphene has been regarded as one of the most promising two-dimensional nanomaterials. Even so, graphene was still faced with several key issues such as impedance mismatching and narrow bandwidth, which have hindered the practical applications of graphene-based nanocomposites in the field of microwave absorption materials. Herein, a series of Si-modified rGO@Fe3O4 composites were investigated and fabricated by a simple method. On one hand, the degree of defects in graphene carbon could be tuned by different silane coupling reagents, which were beneficial to enhancing the dielectric loss. On the other hand, the spherical Fe3O4 nanoparticles provided the magnetic loss resonance, which contributed to controlling the impedance matching. Subsequently, the electromagnetic absorption (EMA) properties of Si-modified rGO@Fe3O4 composites with poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-co-HFP) were investigated in this work. As a result, the Si(2)-rGO@Fe3O4/PVDF-co-HFP composite exhibited the excellent EMA performance in the range of 2–18 GHz. The maximum reflection loss (RLmax) reached −32.1 dB at 3.68 GHz at the thickness of 7 mm and the effective absorption frequency bandwidth for reflection loss (RL) below −10 dB was 4.8 GHz at the thickness of 2 mm. Furthermore, the enhanced absorption mechanism revealed that the high-efficiency absorption performance of Si(2)-rGO@Fe3O4/PVDF-co-HFP composite was attributed to the interference absorption (quarter-wave matching model) and the synergistic effects between Si(2)-rGO@Fe3O4 and PVDF-co-HFP. This work provides a potential strategy for the fabrication of the high-performance EMA materials.

1. Introduction

With the rapid propagation of the electronic devices—especially personal mobile phones, satellite communication, radar detectors, and other communication devices—electromagnetic waves (EMW), taken as “pollution”, are growing to be a huge threat to human health and has been attracted consideration attention [1]. Thus, great efforts have been devoted to exploiting the electromagnetic absorption (EMA) materials with low mass density, ultra-thin, and high EMA performance to eliminate the superfluous EMWs [2,3,4].
In the past decades, metal powders [5], graphite [6], and ferrites [7,8] were the mainstream materials in the field of the EMA materials. However, there are several drawbacks existed in these traditional EMA materials, such as high weight, narrow bandwidth, and unsatisfactory microwave absorption performance, have seriously hindered their practical applications. Nowadays, the carbon-based nanomaterials—such as multi-walled carbon nanotubes (MWCNTs), reduced graphene oxide (rGO), and carbon black—have been given highly attention in the field of aerospace engineering [9,10,11,12]. Particularly, rGO, as one of the most promising carbon-based nanomaterials, is commonly used as a high dielectric material. Because it possesses several excellent characteristics such as being lightweight, and having high specific surface area and abundant surface defects (such as diverse oxygen-containing groups) as well as its excellent mechanical properties. Even so, in terms of EMA impedance principle, pure rGO still is insufficient for impedance matching due to the limitation of single dielectric loss behavior [10,13,14]. Therefore, several scholars have focused on how to adjust the composition of nanomaterial to optimize their electromagnetic (EM) parameters, so as to achieve excellent microwave attenuation. For example, Jin et.al reported the chemical reduction process of rGO by ascorbic acid (VC). It was suggested that the degree of lattice defects in rGO could be tuned by the increase of VC addition, which could significantly enhance the EMA performance [15]. Meng’s group also reported that the nitrogen-doped rGO sheet exhibited the excellent EMA performance in the G band (5.6–8.2 GHz) and X band (8.2–12.4 GHz) due to the existence of the lattice defects in nitrogen-doped rGO [16]. Except for optimizing EM parameters by tuning the degree of defects in rGO, rGO combined with other magnetic loss materials, such as, CoNi [13], CoFe2O4 [17,18], FeCo [18], Fe3O4 [19], and Fe@Fe3O4 [20], is also a meaningful way to control the EMA performance. Particularly, when the magnetically controlled Fe3O4 nanoparticles are directly packaged on the rGO sheet, these results contribute to optimizing the impedance matching and enhance the EMW attenuation [21,22]. Random Fe3O4 nanoparticle packaging can be difficult to predict, thus making it difficult to obtain composite behavior at a large scale [23,24]. Meanwhile, this charge transfer between rGO and magnetic lossy materials can easily generate the interfacial polarization, dipole relaxation, and magnetic loss [25,26].
In general, thermoplastic polymer matrices play an important role in the EMA composites due to their excellent mechanical properties [27,28]. Meanwhile, several interfacial effects or synergetic effects have been constantly occurred between the nano-fillers and thermoplastic polymer matrices, which are available for the enhancement of EMA performance of the absorbers [29,30]. Poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-co-HFP), as a typical dielectric loss material, has been widely applied in the various fields owning to its unique dielectric properties, high mechanical stability and excellent chemical resistance [31,32]. Herein, the fabrication process of two types of Si-modified rGO@Fe3O4/PVDF-co-HFP composites was investigated (Scheme 1). The EMA performance of Si-modified rGO@Fe3O4/PVDF-co-HFP composites could be tuned by different silane groups. Remarkably, the Si(2)-rGO@Fe3O4/PVDF-co-HFP composite achieved the maximum reflection loss (RLmax) value of −32.1 dB (3.68 GHz) at the thickness of 7 mm and the effective absorption frequency bandwidth for reflection loss (RL) below −10 dB was 4.8 GHz at the thickness of 2 mm. Furthermore, the microwave absorption mechanism of Si-modified rGO@Fe3O4/PVDF-co-HFP has been illustrated in detail. Notably, the lattice defects in Si-modified rGO and the synergetic effects of PVDF-co-HFP play an important role in the enhancement of the EMA performance. The analysis of the interference absorption and the impedance matching can also preferably illustrate the high EMA performance of Si-modified rGO@Fe3O4/PVDF-co-HFP composites.

2. Materials and Methods

2.1. Materials

Silane coupling reagents, including (3, 4-epoxycyclohexyl) ethyltrimethoxysilane {Si(1)} and 3-glycidoxypropyldimethoxymethylsilane {Si(2)}, were purchased from Energy Chemical Co., Ltd, Peking, China. Commercial graphene oxide (GO) (1000 mesh) was obtained from Beijing Carbon Century Technology Co., Ltd, Peking, China. Poly (vinylidene fluoride-co-hexafluoropropylene) (PVDF-co-HFP) was provided by Sigma-Aldrich Chemical Company (Sigma-Aldrich (Wuxi) Life Science&Tech. Co., Ltd., Jiangsu, China). Sodium acetate (NaOAc), ethylene glycol (EG), polyethylene glycol (PEG-200), and iron(III) chloride hexahydrate (FeCl3·6H2O) were purchased from Aladdin Chemical Reagent Co., Ltd, Shanghai, China. All chemical reagents were used as received without further purification.

2.2. Preparation of Si-Modified GO

Si-modified GO was fabricated by a silane coupling reagent according to references [33,34]. First, 200 mg GO suspension (1 mg·mL−1 in ethanol) was treated with hydrochloric solution (0.1 M) for pH = 3–4. Afterwards, 10 mL of silane coupling reagent was added into above mixed solution with continuously magnetic stirring at 60 °C for 24 h. After cooling to the room temperature and washed with water and ethanol three times, the Si-modified GO was obtained. The as-produced Si-modified GOs under Si(1) and Si(2) silane coupling reagent were denoted as Si(1)-GO and Si(2)-GO, respectively.

2.3. Preparation of Si-Modified rGO@Fe3O4 Nanocomposites

Si-modified rGO@Fe3O4 nanocomposites were synthesized by the hydrothermal reaction according to literature [35]. First, 90 mg as-obtained Si-modified GO and 900 mg FeCl3·6H2O were dispersed in 5 mL EG by ultrasonically treated for 0.5 h to obtain a homogeneous solution. Second, the above solution was slowly added into the 5 mL of NaOAc solution (0.2 g·mL−1 in EG) at 40 °C for 0.5 h. Third, the homogeneous mixture was transferred into a 50 mL Teflon lined autoclave and heated at 200 °C for 10 h. Finally, the as-prepared Si-modified rGO@Fe3O4 was separated with magnet and washed with ethanol and deionized water 5 times. After drying in 50 °C for 12 h, the Si-modified rGO@Fe3O4 was achieved. According to the silane coupling reagent used, the final products were donated as Si(1)-rGO@Fe3O4, Si(2)-rGO@Fe3O4, respectively. For comparison, rGO@Fe3O4 was also prepared in the existence of Fe3+ and NaOAc.

2.4. Fabrication of Si-Modified rGO@Fe3O4/PVDF-co-HFP Composites

PVDF-co-HFP was first ultrasonically dissolved in 5 mL N, N’-dimethylformamide (DMF) at 40 °C for 1 h. Subsequently, the different mass contents of as-obtained Si-modified rGO@Fe3O4 fillers were added into the above transparent solution and sonicated for 3 h. Finally, the mixture was dried in the vacuum oven at 120 °C for 3 h until the solvent evaporated completely. All samples were compressed into a hollow ring (Φouter: 7.0 mm, Φinner: 3.0 mm) by hot press at 200 °C for 10 min under 10 MPa and then cooling to room temperature naturally. Based on the different mass fractions of Si-modified rGO@Fe3O4 fillers used, the final products were labeled as Si(1)-rGO@Fe3O4/PVDF-co-HFP (S1-x wt %), Si(2)-rGO@Fe3O4/PVDF-co-HFP (S2-x wt %), respectively. x represents the mass fraction of fillers in the composites. For comparison purposes, rGO@Fe3O4/PVDF-co-HFP (S0-x wt %) was also fabricated.

2.5. Characterization

Powder X-ray diffraction (XRD) patterns of the samples were recorded on a Bruker D8 (Bruker AXS, Karlsruhe, Germany) advanced diffractometer using a Cu Kalpha radiation (λ = 0.15405 nm). The morphologies of the samples were investigated by scanning electron microscope (SEM, GeminiSEM 500, Carl Zeiss AG, Oberkochen, Germany) and transmission electron microscopy (TEM, Hitachi HT-7700 at 100 kV, Hitachi Limited, Tokyo, Japan). Fourier transform infrared spectroscopy (FT-IR) was acquired using a Nicolet iS10 FT-IR spectrometer (Thermo Fisher Scientific, Waltham, MA, USA). Raman spectroscopies were studied by a single monochromator with a microscope (Renishaw inVia, Renishaw plc, London, UK) equipped with CCD array detector (1024 × 256 pixels) and an edge filter and 633 nm. X-ray photoelectron spectroscopy (XPS) was measured with a Thermo Fisher Scientific ESCALAB Xi+ spectrometer (Thermo Fisher Scientific, Waltham, MA, USA) equipped with a monochromatic Al Kα radiation. The binding energies were calibrated using the C 1s peak at 284.4 eV. The relative complex EM parameters in the 2–18 GHz frequency were measured by a microwave vector network analyzer (N5227A, Agilent technologies, Santa Clara, CA, USA).

3. Results

3.1. Morphology and Structure

The SEM and TEM images of as-prepared samples are represented in Figure 1 and Figure S1 (Supplementary Materials). When the rGO was decorated by silane coupling reagents, there were more Fe3O4 nanoparticles (NPs) loaded on the surface of Si-modified rGO (Figure 1a,d). The reason is that the existence of –SiOH groups derives from the hydrolysis of –SiOCH3 group within the silane coupling reagent [36], which are preferable to coordinate with Fe3+. Then the Fe3O4 NPs were prepared by in situ reduction. Meanwhile, the spherical Fe3O4 NPs on the Si-modified rGO sheets are featured with rough surface and non-uniform diameters (Figure 1a,b,d,e). As demonstrated in Figure S1 (Supplementary Materials), the composite Si-modified rGO@Fe3O4 still possesses abundant wrinkles as same as that of rGO@Fe3O4 composite, which will benefit for improving the multiple-reflection of EMW [37,38,39]. Furthermore, the SEM images of the Si-modified rGO@Fe3O4/PVDF-co-HFP films illustrate that the Si-modified rGO@Fe3O4 are well dispersive in PVDF-co-HFP (Figure 1c,f).
The analysis of FT-IR and XRD is first devoted to investigating the composition of the Si-modified rGO@Fe3O4 nanocomposites. In most cases, the bands at 1722 cm−1, 1617 cm−1, 1223 cm−1, 1052 cm−1, and 3356 cm−1 are attributed to C=O, C=C, C–O–C, C–OH, and –OH groups in the pure GO, respectively (Figure S2, Supplementary Materials). After modification with silane groups, the stretching vibration of –OH groups decrease obviously and the new peaks at 2918 cm−1 and 2840 cm−1 are observed, corresponding to the vibration of –CH2, –CH3 bond in silane groups. The peaks at about 1037 cm−1 is connected to the Si–O–C (Si–O–Si) bonds (Figure S2, Supplementary Materials), verifying the successful synthesis of Si-modified GO. After in situ hydrothermal reduction, the characteristic peak at 1543 cm−1 belongs to the vibration of C=C bond, suggesting that the Si-modified GO has been successfully reduced to the Si-modified rGO (Figure 2a). Moreover, a new peak at 556 cm−1 is characterized to the stretching vibration of –Fe–O bond in Fe3O4 NPs (Figure 2a). In order to investigate the crystalline structures of as-achieved Si-modified rGO@Fe3O4, the XRD patterns of all the samples are shown in Figure 2b. The broad peak at 2θ = 21.3° is attributed to the (002) facet of rGO [34]. After various silane groups are grafted on the surface of rGO, the diffraction peaks shift to a higher degree around 2θ = 25.1° {Si(1)} and 22.5° {Si(2)}, suggesting that the insertion of the silane group into GO can result in shrinking the d-spacing of the rGO sheet according to the Bragg equation [34]. At the same time, the seven obvious peaks at 18.1°, 30.1°, 35.4°, 43.1°, 53.5°, 56.8°, and 62.5° are assigned to (111), (220), (311), (400), (422), (511), and (440) planes of Fe3O4 NPs (JCPDS file no.19-0629), verifying that the composites contain the phase of Fe3O4 NPs.
To further confirm whether the Fe3O4 NPs is the unique magnetic phase in Si-modified rGO@Fe3O4 nanocomposites, XPS analysis of Fe 2p spectrum is illustrated in Figure 3d. Remarkably, two peaks at 711.5 eV and 725.1 eV is characterized to the Fe 2p 1/2 and Fe 2p 3/2, respectively, and no satellite peak at 719.0 eV indicates no γ-Fe2O3 phase in composites [40,41].
Besides, the XPS analysis also provides an avenue to better understand the chemical valence state of Si-modified rGO@Fe3O4 nanocomposites. For Si-modified GO, there have three elements corresponding to the C, O, and Si elements in the wide span spectra of Si-modified GO (Figure S3a, Supplementary Materials). The four peaks at 284.4 eV, 285.2 eV, 287.2 eV, and 289.3 eV are attributed to the C–C, C–OH, C=O, and C(O)O bonds of GO, respectively (Figure S3b, Supplementary Materials). After modification with silane groups, the intensity of C–C peak of Si(1)-GO obviously increases, whereas its C–OH (285.6 eV) and C=O (287.3 eV) peaks decrease remarkably (Figure S3c, Supplementary Materials). Compared with Si(1)-GO, the intensity of C=O peak of Si(2)-GO is greater than that of Si(1)-GO (Figure S3d, Supplementary Materials), suggesting that the Si(1) is more prone to coupling reaction with –COOH groups in GO. From the Si 2p spectrum of Si(2)-GO (Figure S3e, Supplementary Materials), the peaks at 102.6 eV and 103.5 eV stand for the Si–O–C and Si–O–Si bond, respectively, verifying that most Si(2) reagents have been grafted on the surface of GO and only a part of Si–O–Si groups were obtained by the self-condensation of Si(2) silane coupling reagent [36]. After hydrothermal reduction, there are several oxygen-containing groups still existed in the Si-modified rGO@Fe3O4 composite (Figure 3a,b). Notably, the intensity of C–OH peak of Si(2)-rGO@Fe3O4 is less than that of Si(1)-rGO@Fe3O4. This result reveals that the Si(2)-rGO@Fe3O4 possesses higher reduction degree, which is beneficial for improving the imaginary permittivity of the microwave absorption materials [15]. As shown in Figure 3c, the Si 2p spectrum of Si(2)-rGO@Fe3O4 exhibits the presence of residual –Si–O–C bonds and –Si–O–Si bonds, confirming that several Si(2) silane groups have been existed in Si(2)-rGO@Fe3O4 composite.
It is well known that the lattice defects in the graphene structure are beneficial for enhancing the EMA performance [19]. Here, the influence of various silane groups on rGO defects was investigated by Raman spectroscopy (Figure 3e). Generally, the D-band (1330 cm−1) and G-band (1595 cm−1) represent the lattice defects and the radical C–C stretching vibration of carbon sp2 hybrid in the graphene structure, respectively. The graphitization degree is typically determined by the intensity ratio ID/IG [42]. The higher the ID/IG value, the greater the lattice defects in graphene structure. As revealed in Figure 3e, the ratio ID/IG of rGO@Fe3O4 (1.25) is greater than that of rGO (1.11) due to the introduction of the Fe3O4 NPs. Furthermore, the ID/IG values of Si(1)-rGO@Fe3O4 and Si(2)-rGO@Fe3O4 are 1.47 and 1.62, respectively, implying that the silane group Si(2) grafted on the rGO surface contributes to generating abundant lattice defects in graphene structure.

3.2. Electromagnetic Properties

In most cases, the complex permittivity (ε’ and ε’’) and relative permeability (μ’ and μ’’) are two important EM parameters to judge the quality of the microwave absorption performance. In order to obtain the optimal mass fraction of Si-modified rGO@Fe3O4 in PVDF-co-HFP, the EMW properties of all the samples with different mass fractions loading were investigated in Figure S4–6 (Supplementary Materials). As a result, the Si-modified rGO@Fe3O4 powders with 30 wt % contents in PVDF-co-HFP are the best choice. As shown in Figure 4a,b, the pure PVDF-co-HFP has poor permittivity properties. After addition of fillers, the permittivity values of samples have obvious improved, especially, Si-modified rGO@Fe3O4/PVDF-co-HFP composites possess higher dielectric behavior. The ε’ values of S1 is around 8, and its ε’’ values reach around 2. Similarly, the ε’ values of S2 become around 10 and its ε’’ values are around 3. Based on the free electron theory, ε’’∞σ/2πε0f, where σ stands for the conductivity, it can be found that the S2 sample possesses the higher electrical conductivity, which is attributed to the induced dipoles of the existence of C–O, Si–O species on the surface of S2 composite or vibrations of atoms, ions, or electrons in the S2 composite. Furthermore, the real permeability (μ’) values of S1 and S2 samples are 1.07–0.95 and 1.13–1.01, respectively, which are higher than that of S0 sample without modified by silane groups (about 1.01–0.96) (Figure 4c). Generally, the imaginary permeability (μ’’) values of composites must be more than 0 [43]. As illustrated in Figure 4d, S2 sample is an exception, its μ’’ values show negative in the range of 7–18 GHz frequency. The reason is that the negative μ’’ is attributed to the radiation of the magnetic energy [43]. According to the Maxwell equations [44], the charges transferred in variable electric field is easy to produce the induced magnetic field, which may result in the formation of the magnetic energy [45].
As illustrated in Figure 4e, compared to the dielectric loss tangent (tanδε = ε”/ε’) of the pure PVDF-co-HFP (tanδε = 0.1) and S0 sample (tanδε = 0.3), the higher tanδε values of the Si-modified rGO@Fe3O4/PVDF-co-HFP composites confirm that the silane groups grafted on the rGO surface are more favourable to increase the complex dielectric loss. In particular, S2 sample has the highest tanδε values, corresponding to 0.31–0.38. Furthermore, several resonance peaks in the complex tanδε indicate that the polarization effects may exist in the composites [46]. As shown in Figure 4f, the magnetic loss of samples in the range of 2–13 GHz are greater than that in the range of 13–18 GHz. However, the complex magnetic loss covers weaker values contrast to the dielectric loss. These results suggest that the EMA performance of Si-modified rGO@Fe3O4/PVDF-co-HFP composites is mainly attributed to dielectric loss rather than magnetic loss.
In a general way, the polarization effects of graphene-based composite mainly result from the lattice defects in graphene structure, dipole polarization, or interfacial polarization between rGO and other magnetic metal oxides and polymer matrix, which has an important influence on the complex EMA performance. According to the Cole–Cole semicircle principle, the complex relaxation process can be obtained via Equation (1) [47].
( ε ε s + ε 2 ) 2 + ( ε ) 2 = ( ε s ε 2 ) 2
where ε’ and ε refer to the static dielectric constant and the relative permittivity at boundless frequency, respectively. If Debye relaxation process is occurred in composites, several single semicircles are exhibited in the curve of ε’ and ε” [47,48]. As illustrated in Figure 5a–c, the ε’-ε” plots of pure PVDF-co-HFP is mostly disordered, whereas there is plenty of semicircles in the curve of the samples modified by silane groups, verifying that the dielectric loss of Si-modified rGO@Fe3O4/PVDF-co-HFP composites may result from other multiple interfacial polarizations, including Si-modified rGO@Fe3O4, Fe3O4/PVDF-co-HFP and Si-modified rGO/PVDF-co-HFP interfaces, rather than Debye relaxation [22,49]. Besides, the lattice defects and the dipole polarization in Si-modified rGO@Fe3O4 fillers is also helpful for enhancing the EMA performance of samples decorated by silane groups owning to the existence of C–O, Si–O species on the surface of Si-modified rGO@Fe3O4 composites.
In most cases, the complex magnetic loss usually results from natural resonance, eddy-current effect, and domain-wall displacement [50]. The domain-wall displacement mainly exists in the 1–100 MHz [25,51], suggesting that the EMA performance of Si-modified rGO@Fe3O4/PVDF-co-HFP composites over the range of 2–18 GHz is not attributed to the domain-wall displacement. For the eddy current effect, it can be calculated by Equation (2) [1,52]
C 0 = μ ( μ ) 2 f 1
If the C0 values are equal to the constant in the 2–18 GHz frequency, the complex magnetic loss only arises from the eddy-current [53]. As shown in Figure 5d, the C0 values of all the samples vary with frequency, indicating that the complex magnetic loss behavior over the range of 2–18 GHz frequency is mainly attributed to the natural resonance [53,54].
On the basis of the transmission line theory, the EMA performance of Si-modified rGO@Fe3O4/PVDF-co-HFP composites was illustrated by the RL values, which were calculated by the following equations [47,55,56],
Z i n = Z 0 μ r ε r tanh [ j ( 2 π f d c ) μ r ε r ]
R L = 20 log | Z i n Z 0 Z i n + Z 0 |
where Zin refers to the normalized input impedance, Z0 belongs to the impedance in free space (Z0 = 377 Ω), εr and μr are the complex permittivity and relative permeability, respectively, f is the microwave frequency, d is the thickness of the composite, and c is the velocity of light.
As exhibited in Figure 6a, the pure PVDF-co-HFP at the thickness of 2 mm exhibits poor RL values (RL < −1 dB). After modification with silane groups, the Si-modified rGO@Fe3O4/PVDF-co-HFP composites exhibit the enhanced EMA ability in the range of 2–18 GHz, particularly, the S2 sample modified by Si(2) groups shows high-performance microwave absorption performance in 2–18 GHz frequency. The maximum reflection loss (RLmax) values for S2 sample over the whole frequency range are −17.1 dB at 15.4 GHz. In addition, the S1 sample exhibits the electromagnetic absorption performance over the 18 GHz. Moreover, as shown in Figure 6b–e, the calculated RL values of samples decorated by silane groups in the range of 2–18 GHz are higher than that of pure PVDF-co-HFP and S0 samples without modified by silane groups. The RLmax values for S1 and S2 samples are −27.7 dB at 3.3 GHz with d = 9 mm and −32.1 dB at 3.68 GHz with d = 7 mm, respectively. Meanwhile, S2 sample exhibits a wide absorption frequency bandwidth of 4.8 GHz (RL < −10 dB) at d = 2 mm, demonstrating that Si(2) silane coupling agent is beneficial to improving the EMW absorption broadband of the absorber.
To judge the high-efficiency EMW absorption properties of Si-modified rGO@Fe3O4/PVDF-co-HFP composite in the range of 2–18 GHz, the attenuation constant α, as one of influence factors, can be described by [23,57]
α = 2 π f c × ( μ ε μ ε ) + ( μ ε + μ ε ) 2 + ( μ ε μ ε ) 2
where f refers to the microwave frequency and c refers to the velocity of light. As illustrated in Figure S7 (Supplementary Materials), the S2 sample has the largest attenuation constant values in all the samples in the range of 2–18 GHz, suggesting that the microwave absorption performance of S2 samples is superior to that of S0 and S1 samples over the range of 2–18 GHz. That result is in good agreement with the Figure 6a. Except for the high α values, the impedance matching also plays a significant role in the enhanced microwave attenuation. Here, the modulus of the relative impedances Z = |Zin/Z0| have been calculated by the following Equations (3). When the Z value is almost equal to 1, meaning that the incident EMW can be completely inside the absorber, and then converted into other forms of energy, such as thermal energy [21,58]. As described in Figure S8 (Supplementary Materials), after decoration with silane coupling agent, the Z values of S1 and S2 samples are less than that of S0 sample. Particularly, the Z values in the S2 sample are closer to 1 in the range of 2.6–4 GHz, confirming that the S2 sample exhibits the high-efficiency absorption performance at the thickness of 7–9 mm.
In addition, a quarter-wavelength theory also has been further supplied to explain the EMW absorption principle, the relationship between the thickness (tm) and the relative frequency (fm) can be characterized by equation [47,59,60],
t m = n c / ( 4 f m ( | ε r | | μ r | ) 1 / 2 ) ; n = 1 , 3 , 5 ,
where |εr| and |μr| refers to the modulus of the complex permittivity and relative permeability, respectively. As illustrated in Figure S8 (Supplementary Materials), the black line is the calculated matching thickness (tmfit) and the red spots denote the experimental matching thickness (tmexp). For S2 sample, the values of tmexp almost coincide with that of the tmfit (n = 1), explaining that the excellent EMW performance of S2 sample is mainly attributed to the interference absorption.
Based on the above-mentioned analysis, we have proposed EMA mechanism to explain the reason why S2 sample possesses the high-efficiency absorption ability (Scheme 2). First, after modification with Si(2) silane coupling reagent, there are several dipole polarization in Si(2)-rGO@Fe3O4 fillers owning to the existence of C–O, Si–O group, which is helpful for enhancing the dielectric loss performance (Figure 5c) [14]. Moreover, based on imaginary permittivity analysis of S2-30wt % sample (Figure 4b), the high conductivity results from the Si(2) silane coupling grafted on the surface of rGO. Next, the dielectric loss of S2 sample is also attributed to the complex interfacial polarization (Si(2)-rGO&PVDF-co-HFP, Si(2)-rGO&Fe3O4, and Fe3O4&PVDF-co-HFP) and the lattice defects in graphene structure (Figure 3e), which is beneficial for the EM energy dissipation [16,40]. Meanwhile, the abundant of wrinkles in Si(2)-rGO would provide a channel for improving the multiple-reflection of EMW (Figure S1b,c, Supplementary Materials). Third, permeability parameters (μ’ and μ’’) and Co curve indicated that magnetic loss effect of Fe3O4 NPs in S2 sample mainly resulted from the natural resonance in the range of 2–18 GHz (Figure 5d & Figure S9c, Supplementary Materials). Finally, the synergistic effect of Si(2)-rGO@Fe3O4 and PVDF-co-HFP was beneficial to further improving the microwave absorption properties of S2 sample (Figure 4 & Figure S9, Supplementary Materials), and the absorption interference dominates an important position in the high-efficiency microwave absorption performance of S2 sample (Figure S8, Supplementary Materials).
Moreover, Table 1 also gives the comparison of microwave absorption performance between those in the literature and the obtained Si-modified-rGO@Fe3O4/PVDF-co-HFP, it is clear from the Table 1 that the prepared Si-modified-rGO@Fe3O4/PVDF-co-HFP in this work exhibits primary advantages by fillers loading, effective bandwidth frequency, and effective thickness.

4. Conclusions

In total, a facile method to fabricate series of Si-modified rGO@Fe3O4/PVDF-co-HFP composites was investigated. Meanwhile, the EMW absorption performance of samples illustrated that the lattice defects in graphene modified by silane coupling reagents have a significant influence on the optimized EMA performance. Notably, the optimal Si(2)-rGO@Fe3O4/PVDF-co-HFP with 30 wt % loading (S2-30 wt %) exhibits the high-performance EMA ability. The RLmax value of S2-30 wt % sample over the whole frequency range reaches −32.1 dB at 3.68 GHz at d = 7 mm and its maximum absorption bandwidth for RL < −10 dB is 4.8 GHz (13.2–18 GHz) at a thickness of 2 mm. On the basis of the proposed microwave attenuation mechanism, the high-efficiency EMA performance of S2-30 wt % sample mainly achieves from the interference absorption. Moreover, experimental results highlight that the interfacial polarization, dipole polarization and the higher degree of lattice defects in S2-30 wt % sample and synergistic effect of PVDF-co-HFP is beneficial to improving the dielectric loss. Simultaneously, its magnetic loss mainly originates the natural resonance effects of the Fe3O4 NPs, contributing to achieving the impedance matching. It is undoubtable that construction of Si(2)-rGO@Fe3O4/PVDF-co-HFP composite could provide new possibility and strategy for the fabrication of the high-performance broadband EMA materials.

Supplementary Materials

The following are available online at https://www.mdpi.com/1996-1944/13/4/933/s1, Detailed TEM images of Si-modified rGO@Fe3O4 (Figure S1); FT-IR spectra (Figure S2) and XPS patterns (Figure S3) of Si-modified GO, relative complex (S0–S2) electromagnetic patterns with different mass fraction loading (Figure S4–S6) and complex attenuation constants (Figure S7); |Z| modulus (Figure S8) of Si-modified rGO@Fe3O4/PVDF-co-HFP with 30 wt% loading; and frequency dependence of the electromagnetic parameters of the Si(2)- rGO@Fe3O4/paraffin wax composite (Figure S9).

Author Contributions

Prepared the materials, Y.L. and C.W.; Writing—original draft preparation, Y.L.; Writing—review and editing, Y.D. and Y.L.; Supervision, Y.D.; Data analysis, Y.L. All authors have read and agreed to the published version of the manuscript.

Funding

This funding was funded by the National Natural Science Foundation of China (No. 3112520007).

Acknowledgments

We would like to thank Feng Xiang in Xi’an Jiaotong University who provided the sample tests, Qikui Fan in Xi’an Jiaotong University who tested the TEM images, and Guangbo Chen in Technische Universität Dresden who gave us some advice.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Li, N.; Huang, G.; Li, Y.; Xiao, H.; Feng, Q.; Hu, N.; Fu, S. Enhanced microwave absorption performance of coated carbon nanotubes by optimizing the Fe3O4 nanocoating structure. ACS Appl. Mater. Interfaces 2017, 9, 2973–2983. [Google Scholar] [CrossRef] [PubMed]
  2. Green, M.; Xiang, P.; Liu, Z.; Murowchick, J.; Tan, X.; Huang, F.; Chen, X. Microwave absorption of aluminum/hydrogen treated titanium dioxide nanoparticles. J. Materiomics 2019, 5, 133–146. [Google Scholar] [CrossRef]
  3. Zhang, Y.; Huang, Y.; Zhang, T.; Chang, H.; Xiao, P.; Chen, H.; Huang, Z.; Chen, Y. Broadband and tunable high-performance microwave absorption of an ultralight and highly compressible graphene foam. Adv. Mater. 2015, 27, 2049–2053. [Google Scholar] [CrossRef] [PubMed]
  4. Shi, L.; Zhao, Y.; Li, Y.; Han, X.; Zhang, T. Octahedron Fe3O4 particles supported on 3D MWCNT/graphene foam: In-situ method and application as a comprehensive microwave absorption material. Appl. Surf. Sci. 2017, 416, 329–337. [Google Scholar] [CrossRef]
  5. An, D.; Zhang, Z.; Wang, Y.; Cheng, S.; Liu, Y. The distinctly enhanced electromagnetic wave absorption properties of FeNi/rGO nanocomposites compared with pure FeNi alloys. J. Supercond. Nov. Magn 2019, 32, 385–392. [Google Scholar]
  6. Wu, J.; Chung, D. Improving colloidal graphite for electromagnetic interference shielding using 0.1 um diameter carbon filaments. Carbon 2003, 41, 1313–1315. [Google Scholar] [CrossRef]
  7. Low, K.; Sale, F. Electromagnetic properties of gel-derived NiCuZn ferrites. J. Magn. Magn. Mater. 2002, 246, 30–35. [Google Scholar] [CrossRef]
  8. Kimura, S.; Kato, T.; Hyodo, T.; Shimizu, Y.; Egashira, M. Electromagnetic wave absorption properties of carbonyl iron-ferrite/PMMA composites fabricated by hybridization method. J. Magn. Magn. Mater. 2007, 312, 181–186. [Google Scholar] [CrossRef]
  9. Che, R.; Peng, L.; Duan, X.; Chen, Q.; Liang, X. Microwave absorption enhancement and complex permittivity and permeability of Fe encapsulated within carbon nanotubes. Adv. Mater. 2004, 16, 401–405. [Google Scholar] [CrossRef]
  10. Lv, R.; Kang, F.; Gu, J.; Gui, X.; Wei, J.; Wang, K.; Wu, D. Carbon nanotubes filled with ferromagnetic alloy nanowires: Lightweight and wide-band microwave absorber. Appl. Phys. Lett. 2008, 93, 223105. [Google Scholar] [CrossRef] [Green Version]
  11. Jian, X.; Wu, B.; Wei, Y.; Dou, S.; Wang, X.; He, W.; Mahmood, N. Facile synthesis of Fe3O4/GCs composites and their enhanced microwave absorption properties. ACS Appl. Mater. Interfaces 2016, 8, 6101–6109. [Google Scholar] [CrossRef]
  12. Lv, H.; Yang, Z.; Wang, P.; Ji, G.; Song, J.; Zheng, L.; Zeng, H.; Xu, Z. A voltage-boosting Strategy Enabling a Low-frequency, Flexible Electromagnetic Wave Absorption Device. Adv. Mater. 2018, 30, 1706343. [Google Scholar] [CrossRef] [PubMed]
  13. Duan, Y.; Xiao, Z.; Yan, X.; Gao, Z.; Tang, Y.; Hou, L.; Li, Q.; Ning, G.; Li, Y. Enhanced electromagnetic microwave absorption property of peapod-like MnO@carbon nanowires. ACS Appl. Mater. Interfaces 2018, 10, 40078–40087. [Google Scholar] [CrossRef] [PubMed]
  14. Zhang, X.; Yan, F.; Zhang, S.; Yuan, H.; Zhu, C.; Zhang, X.; Chen, Y. Hollow N-doped carbon polyhedron containing CoNi alloy nanoparticles embedded within few-layer N-doped graphene as high-performance electromagnetic wave absorbing material. ACS Appl. Mater. Interfaces 2018, 10, 24920–24929. [Google Scholar] [CrossRef] [PubMed]
  15. Wang, C.; Han, X.; Xu, P.; Zhang, X.; Du, Y.; Hu, S.; Wang, J.; Wang, X. The electromagnetic property of chemically reduced graphene oxide and its application as microwave absorbing material. Appl. Phys. Lett. 2011, 98, 072906. [Google Scholar] [CrossRef]
  16. Kuang, B.; Song, W.; Ning, M.; Li, J.; Zhao, Z.; Guo, D.; Cao, M.; Jin, H. Chemical reduction dependent dielectric properties and dielectric loss mechanism of reduced graphene oxide. Carbon 2018, 127, 209–217. [Google Scholar] [CrossRef]
  17. Kang, Y.; Chu, Z.; Zhang, D.; Li, G.; Jiang, Z.; Cheng, H.; Li, X. Incorporate boron and nitrogen into graphene to make BCN hybrid nanosheets with enhanced microwave absorbing properties. Carbon 2013, 61, 200–208. [Google Scholar] [CrossRef]
  18. Huang, L.; Li, J.; Wang, Z.; Li, Y.; He, X.; Yuan, Y. Microwave absorption enhancement of porous C@CoFe2O4 nanocomposites derived from eggshell membrane. Carbon 2019, 143, 507–516. [Google Scholar] [CrossRef]
  19. Li, X.; Feng, J.; Du, Y.; Bai, J.; Fan, H.; Zhang, H.; Peng, Y.; Li, F. One-pot synthesis of CoFe2O4/graphene oxide hybrids and their conversion into FeCo/graphene hybrids for lightweight and highly efficient microwave absorber. J. Mater. Chem. A 2015, 3, 5535–5546. [Google Scholar] [CrossRef]
  20. Zhu, C.; Zhang, M.; Qiao, Y.; Xiao, G.; Zhang, F.; Chen, Y. Fe3O4/TiO2 Core/shell nanotubes: synthesis and magnetic and electromagnetic wave absorption characteristics. J. Phys. Chem. C 2010, 114, 16229–16235. [Google Scholar] [CrossRef]
  21. Shu, R.; Zhang, G.; Zhang, J.; Wang, X.; Wang, M.; Gan, Y.; Shi, J.; He, J. Fabrication of reduced graphene oxide/multi-walled carbon nanotubes/zinc ferrite hybrid composites as high-performance microwave absorbers. J. Alloy. Compd. 2018, 736, 1–11. [Google Scholar] [CrossRef]
  22. Li, D.; Liao, H.; Kikuchi, H.; Liu, T. Microporous Co@C nanoparticles prepared by dealloying CoAl@C precursors: achieving strong wideband microwave absorption via controlling carbon shell thickness. ACS Appl. Mater. Interfaces 2017, 9, 44704–44714. [Google Scholar] [CrossRef] [PubMed]
  23. Shorstkii, I.; Yakovlev, N. Synthesis of magnetically controlled Fe3O4 composites and their enhanced microwave absorption properties. Mater. Res. Express 2019, 6, 046104. [Google Scholar] [CrossRef]
  24. Shorstkii, I. Dynamic Arrays Based on Magnetically Controlled Particles: Synthesis and Application. Mat. Res. 2019, 22. [Google Scholar] [CrossRef] [Green Version]
  25. Liu, W.; Liu, J.; Yang, Z.; Ji, G. Extended working frequency of ferrites by synergistic attenuation through a controllable carbothermal route based on Prussian blue shell. ACS Appl. Mater. Interfaces 2018, 10, 28887–28897. [Google Scholar] [CrossRef] [PubMed]
  26. Liang, L.; Han, G.; Li, Y.; Zhao, B.; Zhou, B.; Feng, Y.; Ma, J.; Wang, Y.; Zhang, R.; Liu, C. A promising Ti3C2Tx MXene/Ni chain hybrid with excellent electromagnetic wave absorption and shielding capacity. ACS Appl. Mater. Interfaces 2019, 11, 25399–25409. [Google Scholar] [CrossRef]
  27. Wang, T.; Li, Y.; Geng, S.; Zhou, C.; Jia, X.; Yang, F.; Zhang, L.; Ren, X.; Yang, H. Preparation of flexible reduced graphene oxide/ poly(vinyl alcohol) film with superior microwave absorption properties. RSC Adv. 2015, 5, 88958–88964. [Google Scholar] [CrossRef]
  28. Qin, F.; Brosseau, C. A review and analysis of microwave absorption in polymer composites filled with carbonaceous particles. J. Appl. Phys. 2012, 111, 061301. [Google Scholar] [CrossRef]
  29. Huang, Y.; Yuan, X.; Chen, M.; Song, W.; Chen, J.; Fan, Q.; Tang, L.; Fang, D. Ultrathin Flexible Carbon Fiber Reinforced Hierarchical Metastructure for Broadband Microwave Absorption with Nano Lossy Composite and Multiscale Optimization. ACS Appl. Mater. Interfaces 2018, 10, 44731–44740. [Google Scholar] [CrossRef]
  30. Yang, H.; Han, N.; Lin, Y.; Zhang, G.; Wang, L. Enhanced microwave absorbing properties of PANI/CoFe2O4/PVDF composite. RSC Adv. 2016, 6, 100585–100589. [Google Scholar] [CrossRef]
  31. Xie, D.; Zhang, M.; Wu, Y.; Xiang, L.; Tang, Y. A flexible dual-Ion battery based on sodium-ion quasi-solid-state electrolyte with long cycling life. Adv. Funct. Mater. 2019, 1906770. [Google Scholar] [CrossRef]
  32. Li, H.; Zhang, W.; Ding, Q.; Jin, X.; Ke, Q.; Li, Z.; Wang, D.; Huang, C. Facile Strategy for Fabrication of Flexible, Breathable, and Washable Piezoelectric Sensors via Welding of Nanofibers with Multiwalled Carbon Nanotubes (MWCNTs). ACS Appl. Mater. Interfaces 2019, 11, 38023–38030. [Google Scholar] [CrossRef] [PubMed]
  33. Pan, Y.; Wang, G.; Liu, L.; Liu, L.; Guo, L.; Yu, S. Binary synergistic enhancement of dielectric and microwave absorption properties: A composite of arm symmetrical PbS dendrites and polyvinylidene fluoride. Nano Res. 2017, 10, 284–294. [Google Scholar] [CrossRef]
  34. Guo, L.; Wen, J.; Cheng, G.; Yuan, N.; Ding, J. Synaptic behaviors mimicked in indium-zinc-oxide transistors gated by high-proton-conducting graphene oxide-based composite solid electrolytes. J. Mater. Chem. C 2016, 4, 9762–9770. [Google Scholar] [CrossRef]
  35. Jiang, Y.; Yan, S.; Chen, Y.; Li, S. Preparation, characterization, and properties of silanized graphene oxide reinforced biobased benzoxazine-bismaleimide resin composites. J. Adhes. Sci. Technol. 2019, 33, 1974–1988. [Google Scholar] [CrossRef]
  36. Deng, H.; Li, X.; Peng, Q.; Wang, X.; Chen, J.; Li, Y. Monodisperse magnetic single-crystal ferrite microspheres. Angew. Chem. Int. Edit. 2005, 117, 2842–2845. [Google Scholar] [CrossRef]
  37. Yuan, R.; Ju, P.; Wu, Y.; Ji, L.; Li, H.; Chen, L.; Zhou, H.; Chen, J. Silane-grafted graphene oxide improves wear and corrosion resistance of polyimide matrix: molecular dynamics simulation and experimental analysis. J. Mater. Sci. 2019, 54, 11069–11083. [Google Scholar] [CrossRef]
  38. Tong, Y.; He, M.; Zhou, Y.; Nie, S.; Zhong, X.; Fan, L.; Huang, T.; Liao, Q.; Wang, Y. Three-Dimensional Hierarchical Architecture of the TiO2/Ti3C2Tx/RGO Ternary Composite Aerogel for Enhanced Electromagnetic Wave Absorption. ACS Sustain. Chem. Eng. 2018, 6, 8212–8222. [Google Scholar] [CrossRef]
  39. Kong, L.; Yin, X.; Zhang, Y.; Yuan, X.; Li, Q.; Ye, F.; Cheng, L.; Zhang, L. Electromagnetic wave absorption properties of reduced graphene oxide modified by maghemite colloidal nanoparticle clusters. J. Phys. Chem. C 2013, 117, 19701–19711. [Google Scholar] [CrossRef]
  40. Zong, M.; Huang, Y.; Zhao, Y.; Sun, X.; Qu, C.; Luo, D.; Zheng, J. Facile preparation, high microwave absorption and microwave absorbing mechanism of RGO-Fe3O4 composites. RSC Adv. 2013, 3, 23638–23648. [Google Scholar] [CrossRef]
  41. Wu, H.; Wu, G.; Wang, L. Peculiar porous α-Fe2O3, γ-Fe2O3 and Fe3O4 nanospheres: facile synthesis and electromagnetic properties. Powder Technol. 2015, 269, 443–451. [Google Scholar] [CrossRef]
  42. Zhao, G.; Lv, H.; Zhou, Y.; Zheng, X.; Wu, C.; Xu, C. Self-assembled sandwich-like MXene-derived nanocomposites for enhanced electromagnetic wave absorption. ACS Appl. Mater. Interfaces 2018, 10, 42925–42932. [Google Scholar] [CrossRef] [PubMed]
  43. Chen, T.; Deng, F.; Zhu, J.; Chen, C.; Sun, G.; Ma, S.; Yang, X. Hexagonal and cubic Ni nanocrystals grown on graphene: phase-controlled synthesis, characterization and their enhanced microwave absorption properties. J. Mater. Chem. 2012, 22, 15190–15197. [Google Scholar] [CrossRef]
  44. Liu, Y.; Chen, Z.; Xie, W.; Song, S.; Zhang, Y.; Dong, L. In-situ growth and graphitization synthesis of porous Fe3O4/carbon fiber composites derived from biomass as lightweight microwave absorber. ACS Sustain. Chem. Eng. 2019, 7, 5318–5328. [Google Scholar] [CrossRef]
  45. Deng, L.; Han, M. Microwave absorbing performances of multiwalled carbon nanotube composites with negative permeability. Appl. Phys. Lett. 2007, 91, 023119. [Google Scholar] [CrossRef]
  46. Shi, X.; Cao, M.; Yuan, J.; Fang, X. Dual nonlinear dielectric resonance and nesting microwave absorption peaks of hollow cobalt nanochains composites with negative permeability. Appl. Phys. Lett. 2009, 95, 163108. [Google Scholar] [CrossRef]
  47. Wen, B.; Cao, M.; Hou, Z.; Song, W.; Zhang, L.; Lu, M.; Jin, H.; Fang, X.; Wang, W.; Yuan, J. Temperature dependent microwave attenuation behavior for carbon-nanotube/silica composites. Carbon 2013, 65, 124–139. [Google Scholar] [CrossRef]
  48. Quan, B.; Liang, X.; Zhang, X.; Xu, G.; Ji, G.; Du, Y. Functionalized carbon nanofibers enabling stable and flexible absorbers with effective microwave response at low thickness. ACS Appl. Mater. Interfaces 2018, 10, 41535–41543. [Google Scholar] [CrossRef]
  49. Xie, P.; Li, H.; He, B.; Dang, F.; Lin, J.; Fan, R.; Hou, C.; Liu, H.; Zhang, J.; Ma, Y.; et al. Bio-gel derived nickel/carbon nanocomposites with enhanced microwave absorption. J. Mater. Chem. C 2018, 6, 8812–8822. [Google Scholar] [CrossRef]
  50. Wang, Y.; Zhu, H.; Chen, Y.; Wu, X.; Zhang, W.; Luo, C.; Li, J. Design of hollow ZnFe2O4 microspheres@graphene decorated with TiO2 nanosheets as a high-performance low frequency absorber. Mater. Chem. Phys. 2017, 202, 184–189. [Google Scholar] [CrossRef]
  51. Wu, M.; Zhang, Y.; Hui, S.; Xiao, T.; Ge, S.; Hines, W.; Budnick, J.; Taylor, G. Microwave magnetic properties of Co50/(SiO2)50 nanoparticles. Appl. Phys. Lett. 2002, 80, 4404–4406. [Google Scholar] [CrossRef]
  52. Chen, Y.; Xiao, G.; Wang, T.; Ouyang, Q.; Qi, L.; Ma, Y.; Gao, P.; Zhu, C.; Cao, M.; Jin, H. Porous Fe3O4/carbon core/shell nanorods: synthesis and electromagnetic properties. J. Phys. Chem. C 2011, 115, 13603–13608. [Google Scholar] [CrossRef]
  53. Jian, X.; Xiao, X.; Deng, L.; Tian, W.; Wang, X.; Mahmood, N.; Dou, S. Heterostructured nanorings of Fe−Fe3O4@C hybrid with enhanced microwave absorption performance. ACS Appl. Mater. Interfaces 2018, 10, 9369–9378. [Google Scholar] [CrossRef] [PubMed]
  54. Lv, H.; Zhang, H.; Zhao, J.; Ji, G.; Du, Y. Achieving excellent bandwidth absorption by a mirror growth process of magnetic porous polyhedron structures. Nano Res. 2016, 9, 1813–1822. [Google Scholar] [CrossRef]
  55. Michielssen, E.; Sajer, J.; Ranjithan, S.; Mittra, R. Design of lightweight, broad-band microwave absorbers using genetic algorithms. IEEE Trans. Microw. Theory Tech. 1993, 41, 1024–1031. [Google Scholar] [CrossRef]
  56. Su, Q.; Zhong, G.; Li, J.; Du, G.; Xu, B. Fabrication of Fe/Fe3C-functionalized carbon nanotubes and their electromagnetic and microwave absorbing properties. Appl. Phys. A Mater. Sci. Process 2011, 106, 59–65. [Google Scholar] [CrossRef]
  57. Sun, X.; He, J.; Li, G.; Tang, J.; Wang, T.; Guo, Y.; Xue, H. Laminated magnetic graphene with enhanced electromagnetic wave absorption properties. J. Mater. Chem. C 2013, 1, 765–777. [Google Scholar] [CrossRef]
  58. Wang, R.; He, M.; Zhou, Y.; Nie, S.; Wang, Y.; Liu, W.; He, Q.; Wu, W.; Bu, X.; Yang, X. Self-assembled 3D flower-like composites of heterobimetallic phosphides and carbon for temperature-tailored electromagnetic wave absorption. ACS Appl. Mater. Interfaces 2019, 11, 38361–38371. [Google Scholar] [CrossRef]
  59. Xu, X.; Ran, F.; Fan, Z.; Lai, H.; Cheng, Z.; Lv, T.; Shao, L.; Liu, Y. Cactus-inspired bimetallic metal-organic framework-derived 1D-2D hierarchical Co/N-decorated carbon architecture toward enhanced electromagnetic wave absorbing performance. ACS Appl. Mater. Interfaces 2019, 11, 13564–13573. [Google Scholar] [CrossRef]
  60. Wu, H.; Wu, G.; Ren, Y.; Yang, L.; Wang, L.; Li, X. Co2+/Co3+ Ratio dependence of electromagnetic wave absorption in hierarchical NiCo2O4-CoNiO2 hybrids. J. Mater. Chem. C 2015, 3, 7677–7690. [Google Scholar] [CrossRef]
  61. Xu, W.; Pan, Y.; Wei, W.; Wang, G.; Qu, P. Microwave absorption enhancement and dual-nonlinear magnetic resonance of ultra small nickel with quasi-one-dimensional nanostructure. Appl. Surf. Sci. 2018, 428, 54–60. [Google Scholar] [CrossRef]
  62. Zhang, X.; Li, S.; Wang, S.; Yin, Z.; Zhu, J.; Guo, A.; Wang, G.; Yin, P.; Guo, L. Self-supported construction of three-dimensional MoS2 hierarchical nanospheres with tunable high-performance microwave absorption in broadband. J. Phys. Chem. C 2016, 120, 22019–22027. [Google Scholar] [CrossRef]
  63. Zou, C.; Yao, Y.; Wei, N.; Gong, Y.; Fu, W.; Wang, M.; Jiang, L.; Liao, X.; Yin, G.; Huang, Z.; et al. Electromagnetic wave absorption properties of mesoporous Fe3O4/C nanocomposites. Compos. Part B Eng. 2015, 77, 209–214. [Google Scholar] [CrossRef]
  64. Han, M.; Yin, X.; Kong, L.; Li, M.; Duan, W.; Zhang, L.; Cheng, L. Graphene-wrapped ZnO hollow spheres with enhanced electromagnetic wave absorption properties. J. Phys. Chem. A 2014, 2, 16403–16409. [Google Scholar] [CrossRef]
  65. Liu, P.; Huang, Y.; Sun, X. Excellent Electromagnetic Absorption Properties of Poly(3,4-ethylenedioxythiophene)-Reduced Graphene Oxide-Co3O4 Composites Prepared by a Hydrothermal Method. ACS Appl. Mater. Interfaces 2013, 5, 12355–12360. [Google Scholar] [CrossRef]
  66. Zhu, L.; Liu, N.; Jiang, X.; Yu, L.; Li, X. Four novel 3D RE-MOFs based on maleic hydrazide: Syntheses, structural diversity, efficient electromagnetic wave absorption and antibacterial activity properties. Inorg. Chim. Acta 2020, 501, 119291. [Google Scholar] [CrossRef]
Scheme 1. Schematic diagram of the synthesis procedure of Si-modified rGO@Fe3O4/PVDF-co-HFP composites.
Scheme 1. Schematic diagram of the synthesis procedure of Si-modified rGO@Fe3O4/PVDF-co-HFP composites.
Materials 13 00933 sch001
Figure 1. SEM images of (a,b) Si(1)-rGO@Fe3O4, (c) the film of S1 sample, (d,e) Si(2)-rGO@Fe3O4, (f) the film of S2 sample.
Figure 1. SEM images of (a,b) Si(1)-rGO@Fe3O4, (c) the film of S1 sample, (d,e) Si(2)-rGO@Fe3O4, (f) the film of S2 sample.
Materials 13 00933 g001
Figure 2. FT-IR spectra (a) and XRD patterns (b) of Si-modified rGO@Fe3O4 nanocomposites.
Figure 2. FT-IR spectra (a) and XRD patterns (b) of Si-modified rGO@Fe3O4 nanocomposites.
Materials 13 00933 g002
Figure 3. XPS spectra of Si-modified rGO@Fe3O4: High-resolution C1s spectra of (a) Si(1)-rGO@Fe3O4, (b)Si(2)-rGO@Fe3O4, (c) high resolution Si2p spectrum of Si(2)-rGO@Fe3O4, and (d) Fe2p spectrum of Si(2)-rGO@Fe3O4. (e) Raman spectra of all the samples.
Figure 3. XPS spectra of Si-modified rGO@Fe3O4: High-resolution C1s spectra of (a) Si(1)-rGO@Fe3O4, (b)Si(2)-rGO@Fe3O4, (c) high resolution Si2p spectrum of Si(2)-rGO@Fe3O4, and (d) Fe2p spectrum of Si(2)-rGO@Fe3O4. (e) Raman spectra of all the samples.
Materials 13 00933 g003
Figure 4. Frequency dependence of the EM parameters of all the samples: (a) real permittivity, (b) imaginary permittivity, (c) real permeability, (d) imaginary permeability, (e) dielectric loss, and (f) magnetic loss.
Figure 4. Frequency dependence of the EM parameters of all the samples: (a) real permittivity, (b) imaginary permittivity, (c) real permeability, (d) imaginary permeability, (e) dielectric loss, and (f) magnetic loss.
Materials 13 00933 g004
Figure 5. Cole-cole (ac) and C0 (d) curves for all the samples.
Figure 5. Cole-cole (ac) and C0 (d) curves for all the samples.
Materials 13 00933 g005
Figure 6. Frequency dependence of the calculated RL values of all the samples in the range of 2–18 GHz: (a) the thickness of 2 mm, (be) at different thickness.
Figure 6. Frequency dependence of the calculated RL values of all the samples in the range of 2–18 GHz: (a) the thickness of 2 mm, (be) at different thickness.
Materials 13 00933 g006
Scheme 2. Schematic illustration of the proposed EMA mechanism of S2 sample.
Scheme 2. Schematic illustration of the proposed EMA mechanism of S2 sample.
Materials 13 00933 sch002
Table 1. Comparison of microwave absorption performance of similar composite in the range of 2–18 GHz
Table 1. Comparison of microwave absorption performance of similar composite in the range of 2–18 GHz
SamplesLoading (wt %)RLmax (dB)Thickness (mm)EBDa (GHz)Ref.
Ni/PVDF20−42.0832.5[61]
MoS2/PVDF25−26.112.53.44[62]
Mesoporous Fe3O4/C40−18.02.02.0[63]
Graphene/ZnO50−45.12.22.5[64]
PEDOT/RGO/Co3O4 50−51.12.03.1[65]
[Y2(MH)6]n·DMF20−22.785.02.24[66]
Si(2)-rGO@Fe3O4/PVDF-co-HFP30−17.12.04.8This work
Si(2)-rGO@Fe3O4/PVDF-co-HFP30−32.17.02.88This work
aEBD: Effective bandwidth (RL < −10 dB).

Share and Cite

MDPI and ACS Style

Li, Y.; Duan, Y.; Wang, C. Enhanced Microwave Absorption and Electromagnetic Properties of Si-Modified rGO@Fe3O4/PVDF-co-HFP Composites. Materials 2020, 13, 933. https://doi.org/10.3390/ma13040933

AMA Style

Li Y, Duan Y, Wang C. Enhanced Microwave Absorption and Electromagnetic Properties of Si-Modified rGO@Fe3O4/PVDF-co-HFP Composites. Materials. 2020; 13(4):933. https://doi.org/10.3390/ma13040933

Chicago/Turabian Style

Li, Yuexuan, Yugang Duan, and Chengmeng Wang. 2020. "Enhanced Microwave Absorption and Electromagnetic Properties of Si-Modified rGO@Fe3O4/PVDF-co-HFP Composites" Materials 13, no. 4: 933. https://doi.org/10.3390/ma13040933

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop