Article

Prediction of Temperature Development of Concrete with Set-Controlling Admixture Based on a New Hydration Kinetics Model

1
Materials & Structural Engineering Department, Nanjing Hydraulic Research Institute, Nanjing 210024, China
2
College of Mechanics and Materials, Hohai University, Nanjing 210098, China
3
College of Civil Engineering, Jiangsu Open University, Nanjing 210019, China
*
Author to whom correspondence should be addressed.
Materials 2023, 16(2), 497; https://doi.org/10.3390/ma16020497
Submission received: 21 November 2022 / Revised: 18 December 2022 / Accepted: 24 December 2022 / Published: 4 January 2023

Abstract

:
Temperature control is needed in the construction process of massive concrete and it can avoid the concrete cracks. Prediction of temperature development based on a hydration kinetics model can reduce the need for adiabatic temperature rise tests for concrete. However, the existing hydration kinetics model cannot accurately describe the hydration process of cement, thereby limiting the ability to further accurately predict the temperature rise of concrete based on the hydration kinetics model. This paper aims to establish a new hydration kinetics model, which is based on nucleation and growth model, and to predict the temperature development of concrete with set-controlling admixture based on this model. In this paper, the nucleation and growth of hydration products and the diffusion of free water by the modified boundary of nucleation and growth (BNG) model and the modified Fuji and Kondo’s model are described. The relationship between nucleation rate and apparent activation energy and the relationship between effective diffusion coefficient and apparent activation energy are linear. However, the relationship between growth rate and apparent activation is exponential. Finally, the temperature development of concrete can be calculated by the hydration degree of the cement.

1. Introduction

Recently, bridge engineering, port engineering and water conservancy engineering have involved massive concrete. After pouring massive concrete, temperature stress will be generated due to the influence of the external temperature and the hydration temperature. If the temperature control is insufficient, it will cause concrete cracking, thus threatening the overall safety of the concrete structure. Therefore, temperature control is needed in the construction process of massive concrete. The prediction of temperature development in concrete is essential to control the temperature of the concrete [1,2].
Hydration kinetics of cement has been modeled in many studies since it is the governing process for the prediction of various properties of concrete. Zhang et al. proposed a hydration kinetics model for predicting the degree of hydration at the initial setting time of cement paste with particle agglomeration [3]. Zhang et al. established a new nucleation and growth model and predicted the hydration heat and microstructure of cement with slag by the new model [4]. Wang et al. modified Tomosawa’s hydration kinetics model and predicted the temperature development of concrete incorporating fly ash/slag by the new model [5]. Therefore, an appropriate hydration kinetics model can effectively predict the properties of concrete and reduce a large number of experiments involving concrete in practical engineering.
Several hydration kinetics models have been developed to determine the hydration degree of cement [6,7,8]. There are still two main types of existing hydration kinetics models: single-particle models and nucleation and growth models. However, the existing single-particle models do not account for particle–particle interaction, and do not accurately represent the overall kinetics of a collection of hydrating particles with a wide range of sizes [9,10]. The existing nucleation and growth models do not account for water to cement and particle size distribution of cement [11,12]. Therefore, a new hydration kinetics model must be established to accurately predict the hydration degree of cement.
With the current diversity application requirements of concrete, various admixtures are widely added to the concrete [13]. Set-controlling admixtures, especially, retarders and accelerators, have a significant influence on the hydration of cement [14,15]. However, the effect of set-controlling admixtures on the hydration kinetics of cement is not clear, which makes it is difficult for exiting hydration kinetics to predict the temperature development of concrete mixed with set-controlling admixtures.
This study aimed to establish a hydration kinetics model, which was based on nucleation and growth of products and diffusion of free water. Then, based on the action mechanism of set-controlling admixtures on cement, we modified the hydration kinetics model. Finally, the temperature development of concrete mixed with set-controlling admixtures was predicted by the new hydration kinetics model.

2. Relevant Kinetics Mechanisms and Models

For the hydration kinetics models of cement, Xie et al. [11] summarized in the review article in 2011. They summarized that the kinetics mechanisms of cement included surface reaction, nucleation, growth, space filling, densification and diffusion. The overall hydration process has five main stages in the typical heat-evolution curve. The five main stages are the dissolution period, induction period, acceleration period, deceleration period and slow hydration period. Since the last three periods of cement hydration mainly dominate in the concrete temperature rise, this paper concentrates on studying the acceleration period, deceleration period and slow hydration period. The nucleation and growth of hydration product are deemed to be the driving mechanisms of the acceleration period and the initial part of the deceleration period. Free water diffusion is the driving mechanism of the remaining part of the deceleration and slow hydration periods.

2.1. Boundary Nucleation and Growth

It has been well-accepted that the acceleration period and the initial part of the deceleration period are generated due to nucleation and growth (NG) of hydration products, primarily calcium–silicate–hydrate (C–S–H). To accurately describe the hydration kinetics of cement, there are different hypotheses to the nucleation and growth model.
The Avrami model [16] is a classic homogeneous nucleation model, which assumes that the nucleation of C–S–H randomly takes place on the surface of grains. Subsequently, Cahn [11] suggested a nucleation model for the systems where the nucleation randomly took place on the surface of solids rather than in any available space. Overall, the NG model hypothesizes that the perpendicular impingement explains the transition from acceleration to deceleration with the growing hydration products of neighboring particles. Masoero et al. [17] concluded that the hypothesis of Cahn’s and modified Cahn’s model had a huge flaw, which was that the hypothesis of the NG model did not consider the influence of the water to cement ratio (w/c). Unless the w/c ratio is unusually low, there is enough space for complete hydration. Finally, Masoero et al. [17] proposed a hypothesis to solve the problem: during the early reaction period the C–S–H is restricted to form only within a region close to the cement or C3S particles, which we call the “reaction zone’’. However, many researchers [18,19] using direct microstructural observation found the impingement with the growing hydration products at same particles, but the hypothesis proposed by Masoero et al. neglected that.
Therefore, the existing hypotheses about the nucleation and growth model cannot precisely describe the hydration process of cement. New hypotheses need to be proposed to better fit the hydration kinetics process of cement.

2.2. Diffusion

To explain the behaviors in the slow hydration period, diffusion of free water is deemed to be its driving mechanism. Many works have applied Fuji and Kondo’s model [20] to describe the diffusion period of cement hydration. The mathematical expression of Fuji and Kondo’s model is given in Equation (1).
α = 1 [ ( 1 α ) 1 3 [ 2 D e ( t t * ) ] 1 2 R 0 ] 3
where α is the degree of hydration, R0 is radius of original cement grain, t is the hydration time, t* is the time at which diffusion of water becomes the limiting mechanism, De is the effective diffusion coefficient of water through the C–S–H and De is supposed to be constant.
However, Fuji and Kondo’s model has shortcomings in describing the diffusion period of cement hydration. Firstly, this model assumed that the cement particles were uniform, ignoring the particle size distribution (PSD) effect on the cement hydration. Secondly, this model assumed that the effective diffusion coefficient of water through the C–S–H was constant. However, with the increase of degree of hydration of cement, the porosity and tortuosity of C–S–H was changed, as shown in Figure 1, corresponding to altering the effective diffusion coefficient of water through the C–S–H. Aiming at the above problems, some assumptions of Fuji and Kondo’s model must be reworked.

3. Construction of the New Hydration Kinetics Model

3.1. Nucleation and Growth Model

To solve the shortcomings of the existing models, two assumptions are given: (1) the impingement of hydration products does not only occur on the adjacent particles but also occurs on the adjacent C–S–H nuclei in same particle and (2) the C–S–H product is restricted to form only within a region close to the cement particles, which is called “reaction zone” and we consider that during the early reaction period the adequate free water is the water in the “reaction zone”. The schematic diagram of the derivation process of the nucleation and growth model is given in Figure 2.
Firstly, it is assumed that the growth of C–S–H has different directions. The tangential growth rate is G1 and the normal growth rate of G2, g = G1/G2. The growth in length of the single ellipsoid nucleate in time τ is G2(tτ), then the cross-sectional area A(y) of the single ellipsoid nucleate at the position of the distance y on the cement surface is:
A ( y ) = π g ( G 2 ( t τ ) 2 y 2 )
Then, considering the impingement between the adjacent C–S–H crystal nuclei of the same cement particle, at time t, the actual total cross-sectional area Y(y,t) of the position away from y is:
Y ( y , t ) = 1 exp ( 0 t A ( y ) I ( τ ) d τ )
where I(τ) is nucleation rate. Generally, I(τ) is constant.
Considering the inter-space impingement of different cement particles, the total C–S–H volume VCSH in the cement hydration space can be obtained as follows:
V C S H = V f r e e ( 1 exp ( 0 G 2 t a B V Y ( y , t ) d y ) )
where aBV is the area of the phase boundary per unit volume, which can expressed by:
a B V = S S A V f r e e
where SSA is the specific surface area of cement and Vfree is the volume of effective free water. Here, we consider the free water is the water within “reaction zone”, so the volume of free water can be calculated by:
V f r e e = 0 w ( R 0 ) 4 3 π ( R l i m 3 R 0 3 ) d R 0
where w(R0) is the distribution function of cement, Rlim is the radius of “reaction zone” and R0 is the initial radius of cement particle.
The distribution function of cement particles adopts the Rosin–Rammler distribution function, which can be expressed by:
w ( R 0 ) = m R 0 m 1 R 50 m exp ( ( R 0 R 50 ) m )
where R50 is median particle radius of cement and m is constant.
For the “reaction zone” of cement hydration, Tulio et al. [21] consider that the “reaction zone” is related to initial radius of cement particle and water to cement. The radius of the “reaction zone ” Rlim can be expressed as:
R l i m = R 0 1 + w c ρ c ρ w 3
where w/c is ratio of water to cement, ρc is the density of cement and ρw is the density of water.
The hydration of C3S is assumed to obey the following stoichiometric balance between C3S, water, C–S–H and CH [17]:
C 3 S + 3.1 H C 1.7 SH 1.8 + 1.3 CH
The density and molar volumes of the C3S, water, C–S–H and CH in Equation (9) refer to the Ref. [17]. The densities of four phases are 3.15 g/cm3, 1.00 g/cm3, 2.05 g/cm3 and 2.24 g/cm3, respectively. The molar volumes of four phases are 72.5 cm3/mol, 18.1 cm3/mol, 110.1 cm3/mol and 33.1 cm3/mol, respectively.
The degree of hydration can be calculated according to:
α ( t ) = M C 3 S V f r e e m C 3 S V M C S H ( 1 exp ( 0 G 2 t S S A V f r e e ( 1 exp ( 0 t π g I ( G 2 ( t τ ) 2 y 2 ) d τ ) ) d y ) )
where MC3S is molar mass of C3S, cm3/mol, mC3S is the original mass of C3S, g and VMCSH is molar volume of C–S–H.

3.2. Modified Diffusion Model

3.2.1. Effects of the PSD on Hydration Kinetics

In order to consider the effects of particle size distribution (PSD) on the cement hydration, the degree of hydration for an individual cement particle is αi. The overall degree of hydration αt of the system can be expressed by:
α t = 0 w ( R 0 ) α i d R 0

3.2.2. Effects of the Effective Diffusion Coefficient on Hydration Kinetics

The deposition of C–S–H during the diffusion period of cement hydration will block the pores of C–S–H. Thereby the effective diffusion coefficient of water through the C–S–H changes with the degree of hydration of cement. Park et al. [22,23] considered that the relationship between the effective diffusion coefficient and degree of hydration could be expressed as Equation (3).
D e = k φ D e 0
where De0 is the initial effective diffusion coefficient of water through the C–S–H. kφ is the pore-structure-affecting factor.
To obtain the pore-structure-affecting factor, two assumptions are given: (1) the sedimentation of hydration products on the pores mainly occurs on the pore wall and is evenly deposited layer by layer and (2) the pore of unhydrated cement particle is regarded as a large pore perpendicular to the diffusion direction, which is shown in Figure 1.
Based on above assumption, kφ can be expressed as:
k φ = φ 0 ξ ( d ( x , t ) d 0 ) 2
where ξ is the deflection of the pore, φ0 is the initial porosity, d0 is the initial pore diameter and d(x,t) is the pore diameter corresponding to hydration time t, which is related to the production of C–S–H. The change of pore diameter Δd(x,t) can be expressed as:
Δ d ( x , t ) = d 0 d ( x , t ) = k d ( C c s h C c s h 0 ) d 0
where kd is precipitation constant of C–S–H, Ccsh is the concentration of C–S–H and C0csh is the initial concentration of C–S–H.
Equation (14) can be converted to Equation (15):
d ( x , t ) = d 0 k d ( C c s h C c s h 0 ) d 0
Based on Equation (15), Equation (13) can be converted to Equation (16):
k φ = φ 0 ξ ( 1 k d ( C c s h C c s h 0 ) ) 2
Equation (12) can be converted to Equation (17):
D e = φ 0 τ ( 1 k d ( C c s h C c s h 0 ) ) 2 D e 0
The modified Fuji and Kondo’s model can be expressed as:
α j = 0 w ( R 0 ) ( 1 ( ( 1 α j ) 1 3 ( 2 φ 0 ξ ( 1 k d ( C c s h C c s h 0 ) ) 2 D e 0 ( t t * ) ) 2 R 0 ) d R 0

3.2.3. Effects of Temperature on Hydration Kinetics

As is well known, temperature affects the hydration of cement, which can be analyzed using Arrhenius’s law as follows:
I = I 293 K exp ( E R ( 1 T 1 293 ) )
G = G 293 K exp ( E R ( 1 T 1 293 ) )
D e = D e 293 K exp ( E R ( 1 T 1 293 ) )
where I293K, G293K and De293K are the values of I293K, G293K and De293K at 293K, respectively; E is the apparent activation energy, kJ/mol; R is the gas constant, which is 8.314 J/(mol·K) and T is the curing temperature for hydration of cement, K.

3.2.4. Effects of Cement Composition on Hydration Kinetics

It is assumed that the hydration of C3S plays a main role in the nucleation and growth period. However, each mineral component of cement clinker contributes to the hydration of cement in the diffusion period. The total degree of cement hydration α can be calculated as follows:
α = j = 1 4 α j p j
where αj is the degree of each mineral component of cement clinker hydration, j ∈ {C3S, C2S, C3A, C4AF} and pj is the mass fraction of each mineral components of cement clinker.

3.2.5. Determination of the Transition Time

Ouzia et al. [18] indicated that the inner CSH starts forming at about 20 hand then the mechanism turns into the diffusion period. Zhang et al. [19] have carried out a significant amount of analysis and consider that when the area fraction of the surface covered by outer CSH reaches 99%, the hydration mechanism transforms from nucleation and growth-controlling to diffusion-controlling. In this paper, we assume that the transition in mechanism occurs while V* equals to 99%. Therefore, we can use the following equation solving t*:
V ( t * ) = 1 exp ( 0 G c t * S S A c V f r e e ( 1 exp ( 0 t * π g I c ( G c ( t * τ ) 2 y 2 ) d τ ) ) d y )
Based on the above analysis, the hydration kinetics models of cement can be expressed as following equation.
d α ( t ) d t = { M C 3 S V f r e e m C 3 S V M C S H ( 1 exp ( 0 G 2 t S S A V f r e e ( 1 exp ( 0 t π g I ( G 2 ( t τ ) 2 y 2 ) d τ ) ) d y ) )   t t * j = 1 4 p j d ( 0 w ( R 0 ) ( 1 ( ( 1 α j ) 1 3 ( 2 φ 0 ξ ( 1 k d ( C c s h C c s h 0 ) ) 2 D e 0 ( t t * ) ) 2 R 0 ) d R 0 ) d t   t > t *

3.3. Hydration Kinetics Model for Cement with Set-Controlling Admixture

3.3.1. Influence of Retarder on Cement Hydration

Research carried out over the past 50 years on the mechanisms of action of retarders is summarized in [24,25,26]. There are basically four regimes: (1) calcium complexation preventing precipitation of portlandite, (2) formation of a semipermeable layer preventing hydration, (3) adsorption of retarder on the anhydrous surface and (4) nucleation and growth-poisoning of hydrates. However, this research has found that the action mechanism of retarder seems unlikely to be one of above four regimes. For example, very strong chelators can be moderate retarders while strong retarders can be moderate chelators [27]. In addition, using SEM observation during the induction period, the semipermeable layer cannot be found except in rare hydration products [28].
Yan et al. [29] researched the influence of a temperature-rise inhibitor (TRI) on the hydration of cement, and they found that a TRI not only affected the nucleation and growth of C–S–H but also absorbed onto the cement surface, thereby blocking the surface. Perez et al. [30] used conductimetry and solution analysis to investigate the sodium gluconate retardation to cement, and they concluded that the cement surface formed a adsorbed gluconate layer, approximately 3 nm in thickness. Zajac et al. [31] used quantitative XRD to investigate the influence of retarders (for example, gluconate and tartrate) on the hydration products, and they found that the retarders inhibited the formation of AFt and hydrogarnet.
Based on above analysis, the influence of retarders on the nucleation and growth of hydration products shows in two ways: (1) the retarder occupies the nucleus of hydration products, thereby reducing the rate of nucleation and rate of growth and (2) the retarder blocks the surface of cement, reducing the area of boundary of nucleation and growth.

3.3.2. Influence of Accelerator on Cement Hydration

Due to the variety of accelerators, their mechanism of action is also different. Cheung et al. [24] have summarized the mechanism of action of accelerators. They concluded that a model attempting to describe the interaction of accelerators with cement, must separately deal with: (1) acceleration of pitting on the bare silicate surface during the induction period; (2) acceleration of CH nucleation, which may control saturation levels and affect etch pitting; (3) acceleration of C–S–H nucleation, which affects the reaction rate after the end of induction period and (4) acceleration of C–S–H growth after nucleation. We describe the hydration process after the end of induction period, so the third and fourth questions must be dealt with.
Except for the questions proposed by Cheung et al., many researchers [32,33] found that the dosage of organic accelerators (for example, triethanolamine and triisopropaniamine) over a certain amount inhibits the hydration of cement. Lu et al. [34] studied the influence of triethanolamine on the hydration of cement, and they found that the C3S surface formed a complex layer which inhibited the dissolution of C3S and precipitation of C–S–H during and after the induction period. This research shows that organic accelerators can reduce the area of boundary of nucleation and growth.
Based on the above analysis, the influence of accelerators on the nucleation and growth of hydration products occurs in two ways: (1) accelerators increase the rate of nucleation and rate of growth and (2) organic accelerators can block the surface of cement, reducing the area of boundary of nucleation and growth.

3.3.3. Modified Hydration Kinetics Model

The incorporation of set-controlling admixture alters the rate of nucleation and growth. This paper introduces the nucleation rate effect coefficient Ieff and the growth-rate-effect coefficient Geff. The rate of nucleation Is and rate of growth Gs under the action of set-controlling admixture can be expressed as:
I s = I e f f × I
G s = G e f f × G
The organic set-controlling can adsorb on the surface of cement, reducing the area of the boundary of nucleation and growth. This adsorption property reduces the specific surface area. Therefore, the specific surface area reduction coefficient SSAr is introduced. The specific surface area under the action of set-controlling admixture SSAs can be expressed as:
S S A = S S A r × S S A
Finally, the nucleation and growth model of cement under the action of set-controlling admixture can be expressed as:
d α ( t ) d t = { M C 3 S V f r e e m C 3 S V M C S H d ( 1 exp ( 0 G c t S S A c V f r e e ( 1 exp ( 0 t π g I c ( G c ( t τ ) 2 y 2 ) d τ ) ) d y ) ) d t   t t * j = 1 4 p j d ( 0 w ( R 0 ) ( 1 ( ( 1 α j ) 1 3 ( 2 φ 0 ξ ( 1 k d ( C c s h C c s h 0 ) ) 2 D e 0 ( t t * ) ) 2 R 0 ) d R 0 ) d t   t > t *

4. Predicting Temperature Development of Concrete with Set-Controlling Admixture

4.1. Materials and Methods

4.1.1. Materials

The cement was P.O 42.5 (Chinese standard GB175-2007) ordinary Portland cement (OPC). The detailed oxide compositions of the OPC are shown in Table 1. Citric acid (CA), sodium gluconate (SG), triethanolamine (TEA) and calcium chloride (CC) were chosen as set-controlling admixtures, and their purity was analytically pure.

4.1.2. Methods

The isothermal calorimetry was conducted by an 8-channel TAM Air calorimeter (TA Instruments, New Castle, USA). 10.0 g of the prepared samples with water to binder ratio of 0.5 was used. Isothermal calorimetry of samples was performed at 20 °C for 48 h. The composition of mixes is shown in Table 2.
A small slice about 2 mm thick was taken from the cement paste. The small slice was examined by scanning electron microscope (SEM, FEI Quanta 200, FEI Co., Hillsboro, OR, USA) with an accelerating voltage of 15 kV.
An adiabatic curing test method measures the temperature rise of 50 L of freshly cast concrete. The schematic diagram of an adiabatic temperature rise of concrete testing device are shown in Figure 3. Proportions of concrete mix are given in Table 3.

4.2. Analysis of Hydration Kinetic

The results of fitting using Equation (28) to the calorimetric data of cement with different set-controlling admixtures are shown in Figure 4. The value of hydration kinetics parameters of cement with set-controlling admixture is given in Table 4.
As shown in Table 4, after the cement blending, the retarder, for example, citric acid or sodium gluconate, would reduce the nucleation rate and growth rate of hydration products. Generally, the retarder can complex the Ca2+ to alter the concentration of Ca2+, thereby inhibiting the nucleation of C–S–H. It must be realized that the retarder can adsorb on the surface of cement particles, and reduce the area of boundary of nucleation and growth, thereby reducing the precipitation of C–S–H on the surface. In the diffusion period, the retarder reduces the number of hydration products (Figure 5), and less deposition of hydration products will block the pores, thereby enhancing free water diffusion.
In addition, after the cement blending the accelerator, for example, triethanolamine or calcium chloride, would increase the nucleation rate and growth rate of hydration products. The triethanolamine can promote the dissolution of C3A and C3S, increasing the concentration of Ca2+ and promoting the nucleation and growth of hydration products. The calcium chloride can flocculate hydrophilically, producing a more permeable C–S–H layer around the cement grains at the early hydration stage, promoting the nucleation and growth of hydration products. However, triethanolamine can adsorb on the surface of cement particles, so the addition of triethanolamine must be controlled, or triethanolamine will inhibit the hydration of cement. In the diffusion period, the accelerator increases the number of hydration products (Figure 5), and the greater deposition of hydration products will block the pores, thereby reducing the diffusion of free water.
The relationships between apparent activation energy and nucleation rate (Is), growth rate (Gs) and effective diffusion coefficient (De) are shown in Figure 6. The following rules can be summarized: (1) the nucleation rate increases with the increase of apparent activation energy, and this is a linear relationship; (2) the growth rate increases with the increase of apparent activation energy, and this is an exponential relationship and (3) the effective diffusion coefficient decreases with the increasing of apparent activation energy, and this is a linear relationship.

4.3. Predicting the Adiabatic Temperature Rise History of Concrete

The temperature rise of concrete is caused by the heat release from cement; this increases with the increase of hydration degree. The heat release rate from concrete is related to the mass, composition and hydration rate of cement. The rate of heat release from concrete can be expressed as:
d Q d t = m c H u d α d t
where dQ/dt is rate of heat release from concrete, mc is the mass of cement in concrete, Hu is the ultimate heat release of cement and /dt is the hydration rate of cement.
The ultimate heat release of cement can be calculated by the following empirical formula [35]:
H u = 500 p C 3 S + 260 p C 2 S + 866 p C 3 A + 420 p C 4 A F + 624 p S O 3 + 1186 p f C a O + 850 p M g O
where pC3S, pC2S, pC3A, pC4AF, pSO3, pf-CaO and pMgO are the mass fraction of C3S, C2S, C3A, C4AF, SO3, f-CaO and MgO, respectively.
The heat capacity of concrete is related to the heat capacity of its component. The heat capacity of concrete is calculated by the weighted average of heat capacity of each component, which can be expressed as:
C ( t ) = C c p c + C a p a + C w ( 1 α ) p w
where Cc, Ca and Cw are the heat capacity of cement, aggregate and water, respectively. pc, pa and pw are the mass fraction of cement, aggregate and water, respectively.
The increment temperature rise of concrete can be expressed as:
Δ T = d Q ( t ) C ( t )
The adiabatic temperature rise of concrete can be expressed as:
T = T + d Q ( t ) C ( t )
The flow chart of numerical simulation process is shown in Figure 7. The adiabatic temperature is calculated by Figure 7, and the predicted results is shown in Figure 8.
As shown in Figure 8, the modeled results generally agree with the experimental results. The correlation coefficients and the standard deviation between the modeled results and experimental results for adiabatic temperature rise tests are approximately 0.97 and 2 °C. However, in some cases, such as the concrete with a large amount of calcium chloride, the modeled result shows disagreement with the experimental result. This difference comes from the fact that a large amount of calcium chloride does not evenly act on the cement in the concrete, resulting in the modeled result disagreeing with experimental result.

5. Conclusions

Firstly, based on analysis of the mechanism of cement hydration, a new hydration kinetics model of cement was constructed. Secondly, the hydration kinetics model was used to investigate the influence of set-controlling admixture on cement hydration. Finally, a model of adiabatic temperature rise of concrete was constructed to predict the temperature development of concrete. Based on the model and analysis, the following conclusions are obtained.
  • The influence of retarders on the nucleation and growth of hydration products shows in two ways: (1) the retarder occupies the nucleus of hydration products, thereby reducing the rate of nucleation and rate of growth and (2) the retarder blocks the surface of cement, reducing the area of boundary of nucleation and growth.
  • The influence of accelerators on the nucleation and growth of hydration products shows in two ways: (1) the accelerators increase the rate of nucleation and rate of growth and (2) organic accelerators can block the surface of cement, reducing the area of boundary of nucleation and growth.
  • The nucleation rate increases with the increase of apparent activation energy, and this is a linear relationship. The growth rate increases with the increasing of apparent activation energy, and this is an exponential relationship. The effective diffusion coefficient decreases with the increasing of apparent activation energy, and this is a linear relationship.
  • The hydration rate of cement determines the heat release rate of concrete. Furthermore, the temperature development of concrete can be calculated by the hydration degree of cement and the modeled results agree with the experimental results.
Although we have tried our best to improve the model, there are still some problems to be solved. Firstly, there are too many assumptions in the new hydrtion kinetics model. Our later research will verify our hypothesis through experiments, which will make the new model construction more convincing; secondly, based on the analysis of the mechanism of cement hydration, a new hydration kinetics model of cement was constructed, but merely to predict the temperature development of concrete. Our later research will focus on the prediction of the compressive strength, durability, porosity, etc., of concrete by the new model and check the validity of the model.

Author Contributions

Conceptualization, P.Z. and L.J.; methodology, F.X.; software, Y.S.; validation, F.X., H.C. and M.L.; formal analysis, T.P.; investigation, Y.J.; resources, N.X.; data curation, Y.S.; writing—original draft preparation, Y.Y.; writing—review and editing, P.Z.; visualization, H.C.; supervision, L.J.; project administration, Y.Y.; funding acquisition, P.Z. All authors have read and agreed to the published version of the manuscript.

Funding

The authors would like to acknowledge the financial support of the National Key R&D Program of China (grant No.: 2021YFB2600704); Fundamental Research Funds for Central Public Welfare Research Institutes (Y422007; Y421007; Y422001); the National Key Research and Development Program of China (2018YFC1508704) and the National Natural Science Foundation of China (No. 52078183).

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Not applicable.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Evsukoff, A.G.; Fairbairn, E.M.; Faria, F.; Silvoso, M.M.; Filho, R.D.T. Modeling adiabatic temperature rise during concrete hydration: A data mining approach. Comput. Struct. 2006, 84, 2351–2362. [Google Scholar] [CrossRef]
  2. An, G.-H.; Park, J.-M.; Cha, S.-L.; Kim, J.-K. Development of a portable device and compensation method for the prediction of the adiabatic temperature rise of concrete. Constr. Build. Mater. 2016, 102, 640–647. [Google Scholar] [CrossRef]
  3. Zheng, J.J.; Zhang, J.; Scherer, G.W. Prediction of the degree of hydration at initial setting time of cement paste with particle agglomeration. Cem. Concr. Res. 2012, 42, 1280–1285. [Google Scholar] [CrossRef]
  4. Zhang, Z.; Chen, W.; Han, F.; Yan, P. A new hydration kinetics model of composite cementitious materials, Part 2: Physical effect of SCMs. J. Am. Ceram. Soc. 2020, 103, 3880–3895. [Google Scholar] [CrossRef]
  5. Wang, X.; Lee, H. Modeling the hydration of concrete incorporating fly ash or slag. Cem. Concr. Res. 2010, 40, 984–996. [Google Scholar] [CrossRef]
  6. Liu, K.; Yu, J.; Xia, Y.; Wang, H.; Wang, D.; Du, J.; Tian, Y.; Zhang, X. Quantitative determination of the hydrostatic pressure of oil-well cement slurry using its hydration kinetics. Constr. Build. Mater. 2022, 340, 127704. [Google Scholar] [CrossRef]
  7. Zhou, L.; Gou, M.; Guan, X. Hydration kinetics of cement-calcined activated bauxite tailings composite binder. Constr. Build. Mater. 2021, 301, 124296. [Google Scholar] [CrossRef]
  8. Pang, X.; Sun, L.; Sun, F.; Zhang, G.; Guo, S.; Bu, Y. Cement hydration kinetics study in the temperature range from 15 °C to 95 °C. Cem. Concr. Res. 2021, 148, 106552. [Google Scholar] [CrossRef]
  9. Taplin, J. On the Hydration Kinetics of Hydraulic Cements. In Proceedings of the 5th International Symposium on Chemistry of Cement, Tokyo, Japan, 7–11 October 1968; pp. 337–348. [Google Scholar]
  10. Brown, P. Effects of particle size distribution on the kinetics of hydration of tricalcium silicate. J. Am. Ceram. Soc. 1989, 72, 1829–1832. [Google Scholar] [CrossRef]
  11. Xie, T.; Biernacki, J. The origins and evolution of cement hydration models. Comput. Concr. 2011, 8, 647–675. [Google Scholar] [CrossRef]
  12. Thomas, J.; Biernacki, J.; Bullard, J. Modeling and simulation of cement hydration kinetics and microstructure development. Cem. Conc. Res. 2011, 41, 1257–1278. [Google Scholar] [CrossRef]
  13. Liu, J.; Yu, C.; Shu, X.; Ran, Q.; Yang, Y. Recent advance of chemical admixtures in concrete. Cem. Concr. Res. 2019, 124, 105834. [Google Scholar] [CrossRef]
  14. Teng, Y.; Liu, S.; Zhang, Z. Effect of triethanolamine on the chloride binding capacity of cement paste with a high volume of fly ash. Constr. Build. Mater. 2021, 315, 125612. [Google Scholar] [CrossRef]
  15. Gao, Y.; Guo, T.; Li, Z. Mechanism of retarder on hydration process and mechanical properties of red mud-based geopolymer cementitious materials. Constr. Build. Mater. 2022, 350, 129306. [Google Scholar] [CrossRef]
  16. Avrami, M. Kinetics of phase change. II transformation-time relations for random distribution of nuclei. J. Chem. Phys. 1940, 2, 212–224. [Google Scholar] [CrossRef]
  17. Masoero, E.; Thomas, J.; Jennings, H. A Reaction Zone Hypothesis for the Effects of Particle Size and Water-to-Cement Ratio on the Early Hydration Kinetics of C3S. J. Am. Ceram. Soc. 2013, 97, 967–975. [Google Scholar] [CrossRef] [Green Version]
  18. Ouzia, A.; Scrivener, K. The needle model: A new model for the main hydration peak of alite. Cem. Concr. Res. 2018, 115, 339–360. [Google Scholar] [CrossRef]
  19. Zhang, Z.; Liu, Y.; Huang, L.; Yan, P. A new hydration kinetics model of composite cementitious materials, part 1: Hydration kinetic model of Portland cement. J. Am. Ceram. Soc. 2019, 103, 1970–1991. [Google Scholar] [CrossRef]
  20. Fujii, K.; Kondo, W. Kinetics of the hydration of tricalcium silicate. J. Am. Ceram. Soc. 1974, 11, 492–497. [Google Scholar] [CrossRef]
  21. Honorio, T.; Bary, B.; Benboudjema, F.; Poyet, S. Modeling hydration kinetics based on boundary nucleation and space-filling growth in a fixed confined zone. Cem. Concr. Res. 2016, 83, 31–44. [Google Scholar] [CrossRef]
  22. Park, K.; Noguchi, T.; Plawsky, J. Modeling of hydration reactions using neural networks to predict the average properties of cement paste. Cem. Concr. Res. 2005, 35, 1676–1684. [Google Scholar] [CrossRef]
  23. Park, K.; Jee, N.; Yoon, I.; Lee, H. Prediction of Temperature Distribution in High-Strength Concrete Using Hydration Model. Aci. Mater. J. 2008, 105, 180. [Google Scholar]
  24. Cheung, J.; Jeknavorian, A.; Roberts, L.; Silva, D. Impact of admixtures on the hydration kinetics of Portland cement. Cem. Concr. Res. 2011, 41, 1289–1309. [Google Scholar] [CrossRef]
  25. Previte, R.; W.R. Grace & Co. Some insights on the mechanism of saccharide set retardation of portland cement. Cem. Concr. Res. 1971, 1, 301–316. [Google Scholar] [CrossRef]
  26. Young, J. A review of the mechanisms of set-retardation in portland cement pastes containing organic admixtures. Cem. Concr. Res. 1972, 2, 415–433. [Google Scholar] [CrossRef]
  27. Thomas, N.; Birchall, J. The Retarding Action of Sugars on Cement Hydration. Cem. Concr. Res. 1983, 13, 830–842. [Google Scholar] [CrossRef]
  28. Juilland, P.; Gallucci, E.; Flatt, R.; Scrivener, K. Dissolution Theory Applied to the Induction Period in Alite Hydration. Cem. Concr. Res. 2010, 40, 831–844. [Google Scholar] [CrossRef]
  29. Yan, Y.; Ouzia, A.; Yu, C.; Liu, J.; Scrivener, K. Effect of a novel starch-based temperature rise inhibitor on cement hydration and microstructure development. Cem. Concr. Res. 2020, 129, 105961. [Google Scholar] [CrossRef]
  30. Perez, J.-P. The mechanism of action of sodium gluconate on the fluidity and set of Portland cement. In Proceedings of the 12th International Congress on the Chemistry of Cement, Montreal, QC, Canada, 8–13 July 2007. [Google Scholar]
  31. Zajac, M.; Skocek, J.; Bullerjahn, F.; Haha, M. Effect of retarders on the early hydration of calcium-sulpho-aluminate (CSA) type cements. Cem. Concr. Res. 2016, 84, 62–75. [Google Scholar] [CrossRef]
  32. Yaphary, Y.; Yu, Z.; Lam, R.; Lau, D. Effect of triethanolamine on cement hydration toward initial setting time. Constr. Build. Mater. 2017, 141, 94–103. [Google Scholar] [CrossRef]
  33. Jachiet, M.; Azéma, N.; Le Saoût, G.; Garcia-Diaz, E.; Kocaba, V. Influence of triethanolamine on cement pastes at early age of hydration. Adv. Cem. Res. 2018, 30, 159–171. [Google Scholar] [CrossRef]
  34. Lu, Z.; Kong, X.; Jansen, D.; Zhang, C.; Yin, J. Towards a further understanding of cement hydration in the presence of triethanolamine. Cem. Concr. Res. 2020, 132, 106041. [Google Scholar] [CrossRef]
  35. Riding, K.; Poole, J.; Folliard, K.; Juenger, M.; Schindler, A. Modeling hydration of cementitious systems. Aci. Mater. J. 2012, 109, 225–234. [Google Scholar]
Figure 1. The deposition of CSH during the diffusion period of cement hydration.
Figure 1. The deposition of CSH during the diffusion period of cement hydration.
Materials 16 00497 g001
Figure 2. The schematic diagram of derivation process of nucleation and growth model.
Figure 2. The schematic diagram of derivation process of nucleation and growth model.
Materials 16 00497 g002
Figure 3. Schematic diagram of adiabatic temperature rise of concrete testing device.
Figure 3. Schematic diagram of adiabatic temperature rise of concrete testing device.
Materials 16 00497 g003
Figure 4. The results of fitting using Equation (28) to the calorimetric data of cement with different set-controlling admixtures.
Figure 4. The results of fitting using Equation (28) to the calorimetric data of cement with different set-controlling admixtures.
Materials 16 00497 g004
Figure 5. Microstructure of (a) cement, (b) cement with CA, (c) cement with TEA and (d) cement with CC.
Figure 5. Microstructure of (a) cement, (b) cement with CA, (c) cement with TEA and (d) cement with CC.
Materials 16 00497 g005
Figure 6. The relationship of hydration kinetics parameters between apparent activation energy and (a) Is, (b) Gs and (c) De, respectively.
Figure 6. The relationship of hydration kinetics parameters between apparent activation energy and (a) Is, (b) Gs and (c) De, respectively.
Materials 16 00497 g006
Figure 7. The flow chart of numerical simulation process.
Figure 7. The flow chart of numerical simulation process.
Materials 16 00497 g007
Figure 8. The predicted results of adiabatic temperature rise of concrete with different set-controlling admixtures.
Figure 8. The predicted results of adiabatic temperature rise of concrete with different set-controlling admixtures.
Materials 16 00497 g008
Table 1. The oxide compositions of the cement (%).
Table 1. The oxide compositions of the cement (%).
SiO2Al2O3Fe2O3CaOMgOK2ONa2OSO3Ignition Loss
20.715.293.5562.811.431.10.1671.541.36
Table 2. Composition of mixes (wt.%).
Table 2. Composition of mixes (wt.%).
Sample CodeOPCCASGTEACC
OPC100----
OPC-0.05CA1000.05---
OPC-0.1CA1000.1---
OPC-0.05SG100-0.05--
OPC-0.1SG100-0.1--
OPC-0.05TEA100--0.05-
OPC-0.1TEA100--0.1-
OPC-0.5CC100---0.5
OPC-1CC100---1
Table 3. Proportions of concrete mix (kg/m3).
Table 3. Proportions of concrete mix (kg/m3).
Sample Code WaterOPCFine AggregateCoarse AggregateCASGTEACC
PC214.53908251238----
PC-0.05CA214.539082512380.195---
PC-0.05SG214.53908251238-0.195--
PC-0.05TEA214.53908251238--0.195-
PC-1CC214.53908251238---0.390
Table 4. Hydration kinetics parameters of cement with set-controlling admixture.
Table 4. Hydration kinetics parameters of cement with set-controlling admixture.
Sample CodeIs
(μm−2·h−1)
IeffGs
(μm−2·h−1)
GeffSSAs
(m2·kg−1)
SSArDe
(cm2·h−1)
E/R
(K)
OPC0.022250 1.0000.014580 1.000369.51.0002.87 × 10−86280
OPC-0.05CA0.0194020.8720.0143320.983341.00.9233.56 × 10−85870
OPC-0.1CA0.0148190.6660.0142590.978334.00.9043.89 × 10−85320
OPC-0.05SG0.0197140.8860.0144490.991345.10.9343.23 × 10−85890
OPC-0.1SG0.0165100.7420.0144200.989335.90.9093.67 × 10−85410
OPC-0.05TEA0.0224951.0110.0220891.515359.90.9742.69 × 10−86330
OPC-0.1TEA0.0225621.0140.0250921.721354.40.9592.43 × 10−86450
OPC-0.5CC0.0224281.0080.0323842.907369.51.0002.71 × 10−86310
OPC-1CC0.0225171.0120.0303163.451369.51.0002.55 × 10−86420
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Yu, Y.; Zhu, P.; Shi, Y.; Xu, F.; Jiang, L.; Chu, H.; Xu, N.; Liu, M.; Jia, Y.; Peng, T. Prediction of Temperature Development of Concrete with Set-Controlling Admixture Based on a New Hydration Kinetics Model. Materials 2023, 16, 497. https://doi.org/10.3390/ma16020497

AMA Style

Yu Y, Zhu P, Shi Y, Xu F, Jiang L, Chu H, Xu N, Liu M, Jia Y, Peng T. Prediction of Temperature Development of Concrete with Set-Controlling Admixture Based on a New Hydration Kinetics Model. Materials. 2023; 16(2):497. https://doi.org/10.3390/ma16020497

Chicago/Turabian Style

Yu, Yi, Pengfei Zhu, Yanran Shi, Fei Xu, Linhua Jiang, Hongqiang Chu, Ning Xu, Mingwei Liu, Yu Jia, and Tao Peng. 2023. "Prediction of Temperature Development of Concrete with Set-Controlling Admixture Based on a New Hydration Kinetics Model" Materials 16, no. 2: 497. https://doi.org/10.3390/ma16020497

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop