Article

Superhydrophobic and Corrosion Behaviour of PVDF-CeO2 Composite Coatings

by
Sayed M. Saleh
1,2,*,
Fahad M. Alminderej
1 and
Adel M. A. Mohamed
3,*
1
Department of Chemistry, College of Science, Qassim University, Buraidah 51452, Saudi Arabia
2
Chemistry Branch, Department of Science and Mathematics, Faculty of Petroleum and Mining Engineering, Suez University, Suez 43721, Egypt
3
Department of Metallurgical and Materials Engineering, Faculty of Petroleum and Mining Engineering, Suez University, Suez 43512, Egypt
*
Authors to whom correspondence should be addressed.
Materials 2022, 15(23), 8674; https://doi.org/10.3390/ma15238674
Submission received: 8 November 2022 / Revised: 28 November 2022 / Accepted: 30 November 2022 / Published: 5 December 2022
(This article belongs to the Section Advanced Composites)

Abstract

:
Composite coatings of polyvinylidene fluoride (PVDF)/CeO2 were developed by using the spray approach to explore the wetting and corrosion behaviour of coated materials for applications related to industry. PVDF was combined with different quantities of CeO2 nanoparticles followed by spraying onto glass, aluminium, and steel substrates. The sessile droplet method and microscopy studies were used to assess the wetting behaviour and morphology of the coated surfaces, respectively. The corrosion resistance of uncoated substrates coated with PVDF only was compared with those coated with PVDF/CeO2 nanoparticles through Tafel polarization techniques. In psi, the force of adhesion was measured between the coating layer and the substrates. The PVDF/CeO2-coated steel had a significantly greater water contact angle and lower contact angle hysteresis than coated aluminium and glass substrates, reaching 157 ± 2° and 8 ± 1°, respectively. The corrosion protection efficiency of the superhydrophobic PVDF/CeO2 coatings was considerably higher for steel and aluminium when compared with PVDF coatings. The PVDF/CeO2 coated substrates had modest adhesion between the coating layer and the substrates, but it was still acceptable. Furthermore, the PVDF/CeO2 coatings outperformed PVDF alone in terms of mechanical properties.

1. Introduction

Superhydrophobic surfaces (SHCs) have gained a considerable interest because of their outstanding qualities such as self-cleaning, anti-sticking, and anticontamination [1]. Water repellent, self-cleaning, and corrosion-resistant superhydrophobic coatings having a water contact angle (WCA) higher than 150° have piqued the attention in scientific societies [2]. Because the phenomenon of superhydrophobicity is a result of roughness and surface free energy, two ways for producing SHCs have been proposed: chemically changing a substance’s surface of low surface energy, or increasing the target materials’ surface roughness [3,4,5].
Deposition of chemical vapor [6], hydrothermal-dip coating [7], electrochemical deposition [8], sol gel [9], layer-by-layer self-assembly [10], and polymerization by plasma [11] are some of the techniques for producing rough surfaces with a variety of microstructures that have been documented thus far. For developing the superhydrophobic surfaces having a WCA of more than 150°, many processes were implemented, including hydrothermal growth [12], pulsed laser deposition [13], chemical vapor transport and condensation [14], and spray process [15].
The need for a cost-effective and easier approach for rapid manufacturing of superhydrophobic surfaces has increased, since most of the above procedures require expensive components, more time-consuming manufacturing techniques, and the use of dangerous chemicals. The techniques need high priced components, usage of hazardous chemicals, and gradual and slow fabrication techniques; this gained importance of a clear and simple approach for mass-producing superhydrophobic surfaces that does not cost a lot of money or has limitations should be extensively used.
Spray coating is a cost-effective and straightforward approach for a wide range of applications. It is not bound to a specific type of substrate and can be applied to a large surface area with ease; additionally, it rarely necessitates a more complex and expensive application procedure [16].
Traditionally, polyvinylidene fluoride has been considered to be a hydrophobic material. The thermal and mechanical properties of polyvinylidene fluoride make it suitable for porous polymeric film for use in membrane distillation and filtering [17,18,19]. Even though PVDF has been exposed to numerous methods for enhancing its hydrophobicity to superior levels [20,21], only a few industrial and civil applications of superhydrophobic PVDF-based coatings have been observed. Chaoyi et al. [18], developed a superhydrophobic PVDF coating that possess a WCA and water contact angle hysteresis (WCAH) of 156 ± 1.9 and 2 degrees, respectively, with simple and innovative techniques.
In enhancing the properties of polymers that makes them suitable for particular commercial applications, inorganic nanoparticles such as SiO2 [22,23], TiO2 [12,24], alumina [25] ZnO [26,27], and ZrO2 [28,29] have been used in polymers. A larger fraction of inorganic components is frequently incorporated as a result of these changes.
Among these inorganic components, the low surface energy, surface roughness, and re-entrant structure of CeO2 particles have gained popularity, and all these are vital for attaining hydrophobicity. By combining solid materials such as nickel, cerium, and graphene with the metal oxides such as TiO2, SiO2, ZnO, and CeO2 [30], the surface roughness, which is a parameter of hydrophobicity, can be developed. The toughness and similarity with the organic solvents needed to obtain the PVDF solution have motivated researchers to introduce SiO2 instead of CeO2 (which is frequently used as an integrated particle) to enhance the abrasion strain and scratch [31,32,33]. In this research, the properties of PVDF/CeO2 composite coatings on steel, aluminium, and glass substrates such as wettability, morphology, adhesion, corrosion, and hardness were examined.

2. Experimental Work

2.1. Materials

PVDF polymer (CH2-CF2)n and cerium dioxide (CeO2) nanoparticles of <100 nm particle size were used as raw materials to synthesize PVDF/CeO2 composite coatings. In this study, solvents such as N,N-dimethylformamide (DMF, HCON(CH3)2, >99%, reagent), stearic acid (CH₃-(CH₂)₁₆-COOH), and hexane (C6H14) supplied by the AlSAFWA Centre (Cairo, Egypt) were also employed.

2.2. Preparation of the Coatings

Steel, aluminium, and glass substrates were first cleaned using an ultrasonic cleaner in acetone for 8 min, then distilled water for 8 min, and then they were blown dry in a flow of air before being coated. An amount of 5 g of PVDF was dissolved in DMF at 50 °C and stirred at 500 rpm for 1 h to obtain a homogenous solution. A homogenous dispersion of CeO2 nanoparticles was generated by dispersing different concentrations of CeO2 (1.5, 2, and 2.5 g) in a hexane solution of granules stearic acid and stirring at 500 rpm for 1 h. Obtaining the nanocomposites then required the addition of the CeO2 dispersion solution to the PVDF solution. The final solution was created by vigorous mixing with a magnetic stirrer and mild heating. To achieve a flat surface, the final solution was applied using a spray coating procedure on the cleaned substrates. The coated substrates were then dried for 20 min at 80 °C in a drying furnace. The trial conditions are summarised in Table 1.

2.3. Characterization Methods

At room temperature, the water contact angle (WCA) and water contact angle hysteresis (WCAH) were determined using the sessile droplet method with an Attension Biolin instrument (Model: Theta Optical Tensiometers, Helsinki, Finland). Readings of WCA and WCAH were taken on the coated substrates’ upper surface using 5 µL distilled water droplets. At least five independent determinations made at different places were combined into one sample. The corrosion behaviour of coated steel and aluminium substrates was investigated by measuring Tafel polarisation curves with a VersaSTAT 3 potentiostat/galvanostat (GAMRY, Munich, Germany). A three-electrode cell comprising a working electrode, a graphite counter electrode, and a saturated calomel reference electrode (SCE) at room temperature in 3.5 wt percent NaCl solution at a scan rate of 2 mVs−1 was developed to carry out the corrosion tests. The electrolyte was exposed to 6.25 cm2 of the test sample area. The adhesive force between the coating layer and the substrates was measured using a DeFelsko Digital Pull-off Adhesion Tester (Model: PosiTest AT-M, LANGRY, Shandong, China). With a suitable adhesive (epoxy), every sample was attached to a 20 mm diameter dolly. Thereafter, the combination (dolly + sample) was inserted into a tester, and force was applied to divide them.
The tested samples were sputter coated with Au and vacuum dried prior to morphology analysis. The morphology of the surface for the produced membranes was examined using scanning electron microscopy (SEM Model: JSM-IT200, JOEL, Tokyo, Japan) attached with energy dispersive spectroscopy.

3. Results

3.1. Wettability Results

The existence of solid surface energy can be proved by the contact angles since they are the differentiating parameters between solids and liquids. The best condition’s WCAH, which is the difference between the advancing contact angle and receding contact angle, was also observed. Coating a flat solid surfaces with fluorinated methyl groups leads to a maximum WCA of only 120°, which is too low to be considered superhydrophobic [34]. The wettability of the coating affects its anti-corrosion behaviour, as was studied by several researchers [2,19,25,35,36]. CeO2 nanoparticles were placed on the solid surface to induce superhydrophobicity. The averages of WCA and WCAH values of PVDF-CeO2 composites are shown in Figure 1, Figure 2 and Figure 3.
As shown in Figure 1, the WCA on uncoated steel was about 54 ± 3°, and it was 90 ± 2° when coated with PVDF only, but it climbed to a high of 157 ± 2° upon addition of 2.5 g of CeO2 nanoparticles. WCA was 71 ± 3° on uncoated Al substrates and 91 ± 2° when coated with PVDF only, with an extreme of 147 ± 2° when 2.5 g CeO2 nanoparticles were added, as revealed in Figure 2. WCA on glass substrates was roughly 51 ± 3° prior to coating, 93 ± 2° after coating with PVDF alone, and 155 ± 3° after adding 2.5 g CeO2 nanoparticles, as illustrated in Figure 3. The amount of 2.5 g of CeO2 coating on each substrate exhibited the minimum water contact angle hysteresis (WCAH) ranging from 1 ± 0.5° to 5 ± 1 compared with the uncoated specimens or PVDF alone.
It was suggested to use as an optimal amount the following: For every 100 mL of the final complex solution, 2.5 g of CeO2 can be added to enhance the super hydrophobicity of the PVDF. The decrease in the contact angle hysteresis and increase in the water contact angle was observed and demonstrated as follows. As the amount of CeO2 added increased, the number of nano-sized asperities generated on the surface increased, which increased the layer roughness. In the space between asperities and the liquid droplets, air was trapped by the nanosized asperities that generated a solid–liquid contact surface in the form of water droplets. This discovery bears some resemblance with the Cassie–Baxter hypothesis [1]. The WCA of air was formerly assumed to be 180°. As stated by Cassie–Baxter’s theory, the Yong–Laplace pressure between the interfaces hinders complete contact between liquid droplets and the solid surface; therefore, the asperities trap air in between, resulting in a stable solid–air–liquid three-phase interface [37].
The WCA on a flat surface (θ) and a rough surface (θ’) composed of a solid surface and air [38] can be drawn from Equation (1).
cos ( θ ) = f 1 cos ( θ ) f 2
Here, f1 and f2 are the solid surface and air ratios in contact with liquid, correspondingly. The value of f2 for steel substrates was found to be 0.92, demonstrating that the air was trapped in the roughened hierarchical micro/nanostructures of CeO2, which was the main reason for superhydrophobicity in PVDF-based nanocomposites, based on the WCAs of the flat PVDF film (∼90°) and the PVDF nanocomposite (∼157°). As a result, the larger fraction of air trapped would create a higher WCA after the three phases were stabilized. The WCAH and the WCA are both important elements in determining surface hydrophobicity. It was observed that the increase in CeO2 concentration in the PVDF polymer to 2.5 g/100 mL of the final complex solution enhanced the nanocomposite’s hydrophobicity when the WCAH of the coating film on steel substrates was decreased from 37 ± 2° in the case of PVDF-only coating to only 5 ± 1° after 2.5 g of CeO2 nanoparticles were added (Figure 1),which allows water droplets to easily roll off down the surface.

3.2. Corrosion Analysis

The corrosion resistance of PVDF and PVDF/CeO2 composite coatings was determined using potentiodynamic polarization curves (Tafel). Figure 4 and Figure 5 show the Tafel polarization curves for steel and Al substrates, respectively, for uncoated substrates; PVDF-coated substrates; and PVDF + 1.5, 2, and 2.5 g CeO2-coated substrates at a scan rate of 2 mVs−1 in 3.5 wt. percent NaCl solution. Table 2 provides a summary of the Tafel analysis for the polarization curves.
As seen in Table 2, there was a drastic change in the corrosion current density (icorr) of PVDF alone-coated steel and (PVDF + 2.5 g CeO2)-coated steel from 37.75 in uncoated steel to 3.34 µAcm−2 in PVDF alone-coated steel and 3.08 µAcm−2 (PVDF + 2.5 g CeO2)-coated steel. The icorr of PVDF alone-coated Al and (PVDF + 2.5 g CeO2)-coated Al was reduced from 8.26 (uncoated Al) to 1.3 µAcm−2 (PVDF alone-coated Al) and 0.2 µAcm−2 (PVDF + 2.5 g CeO2)-coated Al). However, the protection efficiency was enhanced to 92% with the improved nanocomposite coating (PVDF + 2.5 g CeO2) from 91% with the PVDF alone. An enhancement in the protection efficiency of Al from 84% (PVDF only) to 97% (PVDF + 2.5 g CeO2) was observed when we improved the nanocomposite coating. Equation (2) gives the protection efficacy of the coatings (η) [39].
η = i 1 i 2 i 1 × 100 %
The corrosion current densities of uncoated and coated substrates, respectively, were i1 and i2.
The values of polarization resistance, Rp, determined using the Stern–Geary equation are also provided in Table 2.
R p = β a β c 2.303 ( β a + β c ) i c o r r
βa and βc are the anodic and cathodic Tafel slopes, respectively, while the polarization resistance is Rp. The Rp value of the superhydrophobic (PVDF + 2.5 g CeO2) was found to be 10 times higher than that of PVDF alone-coated steel, indicating that Rp for the superhydrophobic (PVDF + 2.5 g CeO2) nanocomposite coating was about 10 times greater.
The same was true for Al substrates. When the Rp of the superhydrophobic (PVDF + 2.5 g CeO2) nanocomposite coating was compared to that of the PVDF alone-coated Al, it is clear that the Rp of the superhydrophobic (PVDF + 2.5 g CeO2) nanocomposite coating was 19 times higher.
This means that when coated with (PVDF + 2.5 g CeO2) nanocomposite, both steel and aluminium were much less prone to corrosion than when coated with PVDF alone.
At the polymer surface, gaps were found due to trapped air and the inclusion of CeO2 nanoparticles on the PVDF polymer, which prevented hostile ions from entering the nanocomposite coating [40]. However, when only PVDF was used, the broad pore with low pore resistance allowed aggressive ions to reach the Al surface.

3.3. Adhesion Results

Adhesion is a highly important parameter for the practical application of coatings. Figure 6 depicts the adhesive force of the generated coatings. It is obvious that the adhesion force values for each material of substrate in coated materials followed a similar pattern, with PVDF coatings alone having the highest adherence with the substrates. When CeO2 nanoparticles were introduced, this adhesion was diminished. There were high adhesion forces when they were coated with a low level of nanoparticles (1.5 g CeO2) rather than coatings with high CeO2 concentration.
It is assumed that the high adhesive force of the generated coating surface is mostly due to the effect of cross-linking of PVDF macromolecules through the synthesis of functional groups (C–C or C=C) in the drying process [19]. A decline in the substrate surface’s contact area with the heavy adhesive PVDF was observed by the involved CeO2, which made some nanoparticles settle at the interface between the substrate and coating.
The substrate’s surfaces contact area with the heavy adhesive PVDF decreased with the addition of CeO2, which allowed some nanoparticles to settle at the interface between the substrate and coating, as shown by the bright areas in the crosscut in Figure 7. In terms of adhesive superhydrophobic properties, coatings of (PVDF + 2.5 g CeO2) are preferable, as this combination combines superhydrophobicity with moderate adhesion.

3.4. Coatings’ Surface Morphology

The surface morphology of the generated coatings was investigated using SEM at various magnifications. Figure 8a–c show sponge-like structures in the hydrophobic surface microstructure, showing that the coating layer is predominantly formed of PVDF polymer at high magnification [27,41]. The hydrophobic sample has a uniform surface structure with slight roughness. There are other massive microvoids beyond these formations. Figure 8c shows how EDS was utilised to check the composition of PVDF polymer. According to EDS studies, PVDF material consists mostly of two fluorine (F) and carbon (C) peaks.
As indicated by the bright areas in Figure 9, the addition of CeO2 nanoparticles resulted in a considerable change in morphology (a–c). The composite coatings were comprised of CeO2 particle aggregates, as seen in Figure 9a. As shown in Figure 9c, the micro–nano scale structured roughness surfaces were made from CeO2 particles with a variety of morphologies. This micro–nano scale structure aids the film’s superhydrophobicity, which has a static WCA of 157 ± 2° and a WCAH of 5 ± 1°. The EDS spectrums in Figure 9d reveal the main chemical components of the samples comprising (PVDF + 2.5 g CeO2). The PVDF structure had carbon and fluorine, but the integrated CeO2 structure contained cerium (Ce) and oxygen (O). EDS elemental analysis of the coated surfaces is shown in Table 3.

4. Conclusions

The following are some possible conclusions based on the preceding discussion:
  • PVDF/CeO2 composites were successfully made using spray coating processes. This technology has the potential to be employed in wide-scale procedures and to be a cheap solution for industrial applications.
  • The superhydrophobicity of PVDF/CeO2 composite coatings is due to the PVDF’s low surface energy and the mixing of hierarchical micro and nanostructures of CeO2 incorporated in the polymer.
  • If we raise the concentration of CeO2 nanoparticles to 2.5 g/100 mL, the complex solution on the steel surface in the PVDF matrix obtained a considerable increase of WCA from 90 ± 2° to 157 ± 2°, with a fall in WCAH to 5 ± 1°. Both Al and glass substrates produced similar results.
  • By minimizing the size of pores in the composite coating and raising air trapping within the surface’s gaps, CeO2 nanoparticles improve the hydrophobicity of PVDF coatings.
  • A significant enhancement in the corrosion resistance of the superhydrophobic PVDF/CeO2 composite coatings was observed as 77 times less than the uncoated steel and 177 times lower than the Al substrate. The corrosion rates of the prepared PVDF coating without CeO2 nanoparticles were 71 times less than on steel and 44 times lower than on the Al substrates.
  • Although PVDF alone has a stronger adhesive force than (PVDF + 2.5 g CeO2) composite coatings, the composite’s adherence is acceptable.

Author Contributions

Conceptualization, A.M.A.M.; methodology, S.M.S., A.M.A.M. and F.M.A.; formal analysis, A.M.A.M. and S.M.S.; investigation, A.M.A.M. and F.M.A.; resources, F.M.A.; data curation, A.M.A.M. and S.M.S.; writing—original draft preparation, A.M.A.M. and S.M.S.; writing—review and editing, A.M.A.M.; supervision, A.M.A.M. and S.M.S. All authors have read and agreed to the published version of the manuscript.

Funding

The authors extend their appreciation to the Deputyship for Research and Innovation, Ministry of Education, Saudi Arabia, for funding this research work through the project number (QU-IF-4-5-1-29871). The authors also thank Qassim University for technical support.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Data sharing is not applicable to this article.

Acknowledgments

The authors extend their appreciation to the Deputyship for Research and Innovation, Ministry of Education, Saudi Arabia, for funding this research work through the project number (QU-IF-4-5-1-29871). The authors also thank Qassim University for technical support.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Mohamed, A.M.A.; Jafari, R.; Farzaneh, M. An optimization of superhydrophobic polyvinylidene fluoride/zinc oxide materials using Taguchi method. Appl. Surf. Sci. 2014, 288, 229–237. [Google Scholar] [CrossRef]
  2. Radwan, A.B.; Mohamed, A.M.A.; Abdullah, A.M.; Al-Maadeed, M.A. Corrosion protection of electrospun PVDF-ZnO superhydrophobic coating. Surf. Coat. Technol. 2016, 289, 136–143. [Google Scholar] [CrossRef]
  3. Qian, B.; Shen, Z. Fabrication of superhydrophobic surfaces by dislocation-selective chemical etching on aluminum, copper, and zinc substrates. Langmuir 2005, 21, 9007–9009. [Google Scholar] [CrossRef] [PubMed]
  4. Burkarter, E.; Saul, C.K.; Thomazi, F.; Cruz, N.C.; Zanata, S.M.; Roman, L.S.; Schreiner, W.H. Electrosprayed superhydrophobic PTFE: A non-contaminating surface. J. Phys. D Appl. Phys. 2007, 40, 7778–7781. [Google Scholar] [CrossRef]
  5. Meng, L.Y.; Park, S.J. Effect of fluorination of carbon nanotubes on superhydrophobic properties of fluoro-based films. J. Colloid Interface Sci. 2010, 342, 559–563. [Google Scholar] [CrossRef] [PubMed]
  6. Huang, L.; Lau, S.P.; Yang, H.Y.; Leong, E.S.P.; Yu, S.F.; Prawer, S. Stable superhydrophobic surface via carbon nanotubes coated with a ZnO thin film. J. Phys. Chem. B 2005, 109, 7746–7748. [Google Scholar] [CrossRef]
  7. Gan, W.Y.; Lam, S.W.; Chiang, K.; Amal, R.; Zhao, H.; Brungs, M.P. Novel TiO2 thin film with non-UV activated superwetting and antifogging behaviours. J. Mater. Chem. 2007, 17, 952–954. [Google Scholar] [CrossRef]
  8. Nicolas, M.; Guittard, F.; Géribaldi, S. Stable superhydrophobic and lipophobic conjugated polymers films. Langmuir 2006, 22, 3081–3088. [Google Scholar] [CrossRef]
  9. Taurino, R.; Fabbri, E.; Messori, M.; Pilati, F.; Pospiech, D.; Synytska, A. Facile preparation of superhydrophobic coatings by sol-gel processes. J. Colloid Interface Sci. 2008, 325, 149–156. [Google Scholar] [CrossRef]
  10. Amigoni, S.; De, E.T.G.; Dufay, M.; Guittard, F. Covalent layer-by-layer assembled superhydrophobic organic-inorganic hybrid films. Langmuir 2009, 25, 11073–11077. [Google Scholar] [CrossRef]
  11. Chen, W.; Fadeev, A.Y.; Hsieh, M.C.; Öner, D.; Youngblood, J.; McCarthy, T.J. Ultrahydrophobic and ultralyophobic surfaces: Some comments and examples. Langmuir 1999, 15, 3395–3399. [Google Scholar] [CrossRef]
  12. Liu, Z.; Zhang, C.; Zhang, X.; Wang, C.; Liu, F.; Yuan, R.; Wang, H. Durable superhydrophobic PVDF/FEVE/GO@TiO2 composite coating with excellent anti-scaling and UV resistance properties. Chem. Eng. J. 2021, 411, 128632. [Google Scholar] [CrossRef]
  13. Roach, P.; Shirtcliffe, N.J.; Newton, M.I. Progess in superhydrophobic surface development. Soft Matter 2008, 4, 224. [Google Scholar] [CrossRef] [PubMed]
  14. Song, X.; Zhai, J.; Wang, Y.; Jiang, L. Fabrication of Superhydrophobic Surfaces by Self-Assembly and Their Water-Adhesion Properties. J. Phys. Chem. B 2005, 109, 4048–4052. [Google Scholar] [CrossRef] [PubMed]
  15. Xue, C.-H.; Jia, S.-T.; Zhang, J.; Ma, J.-Z. Large-area fabrication of superhydrophobic surfaces for practical applications: An overview. Sci. Technol. Adv. Mater. 2010, 11, 033002. [Google Scholar] [CrossRef]
  16. Yang, J.; Zhang, Z.; Men, X.; Xu, X.; Zhu, X. A simple approach to fabricate regenerable superhydrophobic coatings. Colloids Surfaces A Physicochem. Eng. Asp. 2010, 367, 60–64. [Google Scholar] [CrossRef]
  17. Zhang, W.; Shi, Z.; Zhang, F.; Liu, X.; Jin, J.; Jiang, L. Superhydrophobic and superoleophilic PVDF membranes for effective separation of water-in-oil emulsions with high flux. Adv. Mater. 2013, 25, 2071–2076. [Google Scholar] [CrossRef]
  18. Peng, C.; Xing, S.; Yuan, Z.; Xiao, J.; Wang, C.; Zeng, J. Preparation and anti-icing of superhydrophobic PVDF coating on a wind turbine blade. Appl. Surf. Sci. 2012, 259, 764–768. [Google Scholar] [CrossRef]
  19. Wang, H.; Liu, Z.; Wang, E.; Yuan, R.; Gao, D.; Zhang, X.; Zhu, Y. A robust superhydrophobic PVDF composite coating with wear/corrosion-resistance properties. Appl. Surf. Sci. 2015, 332, 518–524. [Google Scholar] [CrossRef]
  20. Zhang, H.; Guo, Y.; Zhang, X.; Hu, X.; Wang, C.; Yang, Y. Preparation and characterization of PSF-TiO2 hybrid hollow fiber UF membrane by sol-gel method. J. Polym. Res. 2020, 27, 376. [Google Scholar] [CrossRef]
  21. Shang, H.M.; Wang, Y.; Takahashi, K.; Cao, G.Z.; Li, D.; Xia, Y.N. Nanostructured superhydrophobic surfaces. J. Mater. Sci. 2005, 40, 3587–3591. [Google Scholar] [CrossRef]
  22. Tan, X.; Huang, Z.; Jiang, L.; Xiao, T.; Wang, Y.; Yang, Y.; Zhu, H.; Li, S.; Chen, X. A simple fabrication of superhydrophobic PVDF/SiO2 coatings and their ant-icing properties. J. Mater. Res. 2021, 210, 637–645. [Google Scholar] [CrossRef]
  23. Liu, Z.; Wang, H.; Zhang, X.; Lv, C.; Zhao, Z.; Wang, C. Durable and self-healing superhydrophobic polyvinylidene fluoride (PVDF) composite coating with in-situ gas compensation function. Surf. Coat. Technol. 2017, 327, 18–24. [Google Scholar] [CrossRef]
  24. Qing, Y.; Yang, C.; Yu, N.; Shang, Y.; Sun, Y.; Wang, L.; Liu, C. Superhydrophobic TiO2/polyvinylidene fluoride composite surface with reversible wettability switching and corrosion resistance. Chem. Eng. J. 2016, 290, 37–44. [Google Scholar] [CrossRef]
  25. Ghazali, N.; Basirun, W.J.; Nor, A.M.; Johan, M.R. Super-amphiphobic coating system incorporating functionalized nano-Al2O3 in polyvinylidene fluoride (PVDF) with enhanced corrosion resistance. Coatings 2020, 10, 387. [Google Scholar] [CrossRef] [Green Version]
  26. Liu, Z.; Wang, H.; Wang, E.; Zhang, X.; Yuan, R.; Zhu, Y. Superhydrophobic poly(vinylidene fluoride) membranes with controllable structure and tunable wettability prepared by one-step electrospinning. Polymer 2016, 82, 105–113. [Google Scholar] [CrossRef]
  27. Hong, J.; He, Y. Effects of nano sized zinc oxide on the performance of PVDF microfiltration membranes. Desalination 2012, 302, 71–79. [Google Scholar] [CrossRef]
  28. Wei, X.L.; Li, N.; Yi, W.J.; Li, L.J.; Chao, Z.S. High performance super-hydrophobic ZrO2-SiO2 porous ceramics coating with flower-like CeO2 micro/nano-structure. Surf. Coat. Technol. 2017, 325, 565–571. [Google Scholar] [CrossRef]
  29. Duan, Z.; Luo, D.; Liu, Z.; Zhao, Z.; Zhao, M.; Zhang, J.; Zhao, G. Patterning ZrO2 films surface: Superhydrophilic and superhydrophobic properties. Ceram. Int. 2017, 43, 5089–5094. [Google Scholar] [CrossRef]
  30. Latthe, S.S.; Gurav, A.B.; Maruti, C.S.; Vhatkar, R.S. Recent Progress in Preparation of Superhydrophobic Surfaces: A Review. J. Surf. Eng. Mater. Adv. Technol. 2012, 2, 76–94. [Google Scholar]
  31. Lakshmi, R.V.; Bharathidasan, T.; Bera, P.; Basu, B.J. Fabrication of superhydrophobic and oleophobic sol-gel nanocomposite coating. Surf. Coat. Technol. 2012, 206, 3888–3894. [Google Scholar] [CrossRef]
  32. Xiong, D.; Liu, G.; Duncan, E.J.S. Robust amphiphobic coatings from bi-functional silica particles on flat substrates. Polymer 2013, 54, 3008–3016. [Google Scholar] [CrossRef]
  33. Hsieh, C.T.; Wu, F.L.; Chen, W.Y. Superhydrophobicity and superoleophobicity from hierarchical silica sphere stacking layers. Mater. Chem. Phys. 2010, 121, 14–21. [Google Scholar] [CrossRef]
  34. Basu, B.J.; Kumar, V.D.; Anandan, C. Surface studies on superhydrophobic and oleophobic polydimethylsiloxane- silica nanocomposite coating system. Appl. Surf. Sci. 2012, 261, 807–814. [Google Scholar] [CrossRef]
  35. Wei, J.; Li, B.; Jing, L.; Tian, N.; Zhao, X.; Zhang, J. Efficient protection of Mg alloy enabled by combination of a conventional ant-corrosion coating and a superamphiphobic coating. Chem. Eng. J. 2020, 390, 124562–124575. [Google Scholar] [CrossRef]
  36. Wang, N.; Xiong, D. Applied Surface Science Superhydrophobic membranes on metal substrate and their corrosion protection in different corrosive media. Appl. Surf. Sci. 2014, 305, 603–608. [Google Scholar] [CrossRef]
  37. Dhoke, S.K.; Khanna, A.S. Electrochemical impedance spectroscopy (EIS) study of nano-alumina modified alkyd based waterborne coatings. Prog. Org. Coat. 2012, 74, 92–99. [Google Scholar] [CrossRef]
  38. Kang, M.; Jung, R.; Kim, H.S.; Jin, H.J. Preparation of superhydrophobic polystyrene membranes by electrospinning. Colloids Surfaces A Physicochem. Eng. Asp. 2008, 313–314, 411–414. [Google Scholar] [CrossRef]
  39. Mohamed, A.M.A.; Abdullah, A.M.; Younan, N.A. Corrosion behavior of superhydrophobic surfaces: A review. Arab. J. Chem. 2015, 8, 749–765. [Google Scholar] [CrossRef] [Green Version]
  40. Nakajima, A.; Hashimoto, K.; Watanabe, T. Recent Studies on Super-Hydrophobic Films. In Molecular Materials and Functional Polymers; Springer: Vienna, Austria, 2001; Volume 41, pp. 31–41. [Google Scholar]
  41. el Haleem, S.M.A.; el Wanees, S.A.; Bahgat, A. Environmental factors affecting the corrosion behaviour of reinforcing steel. VI. Benzotriazole and its derivatives as corrosion inhibitors of steel. Corros. Sci. 2014, 87, 321–333. [Google Scholar] [CrossRef]
Figure 1. Surface wetting of S1, S2, S3, S4, and S5 samples (steel substrates).
Figure 1. Surface wetting of S1, S2, S3, S4, and S5 samples (steel substrates).
Materials 15 08674 g001
Figure 2. Surface wetting of A1, A2, A3, A4, and A5 samples (Al substrates).
Figure 2. Surface wetting of A1, A2, A3, A4, and A5 samples (Al substrates).
Materials 15 08674 g002
Figure 3. Surface wetting of G1, G2, G3, G4, and G5 samples (glass substrates).
Figure 3. Surface wetting of G1, G2, G3, G4, and G5 samples (glass substrates).
Materials 15 08674 g003
Figure 4. Tafel curves of uncoated steel, PVDF-coated steel, and coated steel with varying CeO2 contents of coatings (1.5, 2, and 2.5 g) in a 3.5 percent NaCl solution and a scan rate of 2 mVs−1.
Figure 4. Tafel curves of uncoated steel, PVDF-coated steel, and coated steel with varying CeO2 contents of coatings (1.5, 2, and 2.5 g) in a 3.5 percent NaCl solution and a scan rate of 2 mVs−1.
Materials 15 08674 g004
Figure 5. Tafel curves of uncoated Al, PVDF-coated Al, and coated Al with varying CeO2 contents of coatings (1.5, 2, and 2.5 g) in a 3.5 percent NaCl solution at a scan rate of 2 mVs−1.
Figure 5. Tafel curves of uncoated Al, PVDF-coated Al, and coated Al with varying CeO2 contents of coatings (1.5, 2, and 2.5 g) in a 3.5 percent NaCl solution at a scan rate of 2 mVs−1.
Materials 15 08674 g005
Figure 6. Force of adhesion between (a) steel, (b) Al, and (c) glass substrates, and PVDF alone and PVDF + CeO2 coatings.
Figure 6. Force of adhesion between (a) steel, (b) Al, and (c) glass substrates, and PVDF alone and PVDF + CeO2 coatings.
Materials 15 08674 g006
Figure 7. Crosscut SEM images of PVDF composites containing 2.5 g CeO2 with nanoparticles on the interface.
Figure 7. Crosscut SEM images of PVDF composites containing 2.5 g CeO2 with nanoparticles on the interface.
Materials 15 08674 g007
Figure 8. (ac) PVDF alone coatings at various magnifications and (d) EDS peaks of point 1 in image (c).
Figure 8. (ac) PVDF alone coatings at various magnifications and (d) EDS peaks of point 1 in image (c).
Materials 15 08674 g008aMaterials 15 08674 g008b
Figure 9. (ac) SEM images of PVDF composites containing 2.5 g CeO2 at various magnifications and (d) EDS peaks of point 1 in image (c).
Figure 9. (ac) SEM images of PVDF composites containing 2.5 g CeO2 at various magnifications and (d) EDS peaks of point 1 in image (c).
Materials 15 08674 g009aMaterials 15 08674 g009b
Table 1. Conditions of the experiments.
Table 1. Conditions of the experiments.
SubstrateCoatingWt/100 mL of
Composite Solution
Substrate Code
SteelUncoated-S1
PVDF5.0 gS2
CeO21.5 gS3
2.0 gS4
2.5 gS5
AluminiumUncoated-A1
PVDF5.0 gA2
CeO21.5 gA3
2.0 gA4
2.5 gA5
GlassUncoated-G1
PVDF5.0 gG2
CeO21.5 gG3
2.0 gG4
2.5 gG5
Table 2. Tafel analysis of uncoated substrates, PVDF alone, and composite coatings (PVDF + 2.5 g CeO2) after immersion in a 3.5 percent NaCl aqueous solution; 2 mVs−1 was the scan rate.
Table 2. Tafel analysis of uncoated substrates, PVDF alone, and composite coatings (PVDF + 2.5 g CeO2) after immersion in a 3.5 percent NaCl aqueous solution; 2 mVs−1 was the scan rate.
Steel Substratesβa (mV)βc (mV)Rp
(K Ω cm2)
CR Rate (mpy) i c o r r ( µ A / cm 2 ) η (%)
Uncoated Steel1171390.71737.75-
PVDF731986.90.243.3491
PVDF + 2.5 g CeO253868942.60.223.0892
Aluminium Substratesβa (mV)βc (mV)Rp
(K Ω cm2)
CR Rate (mpy) i c o r r (µA/cm2)η(%)
Uncoated Aluminium541221.93.548.26-
PVDF93865280.081.384
PVDF + 2.5 g CeO23836585250.020.297
Table 3. EDS analysis of surface components on an Al substrate for PVDF alone and (PVDF + 2.5 g CeO2) composite coatings.
Table 3. EDS analysis of surface components on an Al substrate for PVDF alone and (PVDF + 2.5 g CeO2) composite coatings.
ElementPVDF OnlyPVDF + 2.5 g CeO2
Mass %Atom %Mass %Atom %
C55.8059.3533.1853.52
F44.2040.6524.9025.40
O--14.2517.25
Ce--27.673.83
Total100.00100.00100.00100.00
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Saleh, S.M.; Alminderej, F.M.; Mohamed, A.M.A. Superhydrophobic and Corrosion Behaviour of PVDF-CeO2 Composite Coatings. Materials 2022, 15, 8674. https://doi.org/10.3390/ma15238674

AMA Style

Saleh SM, Alminderej FM, Mohamed AMA. Superhydrophobic and Corrosion Behaviour of PVDF-CeO2 Composite Coatings. Materials. 2022; 15(23):8674. https://doi.org/10.3390/ma15238674

Chicago/Turabian Style

Saleh, Sayed M., Fahad M. Alminderej, and Adel M. A. Mohamed. 2022. "Superhydrophobic and Corrosion Behaviour of PVDF-CeO2 Composite Coatings" Materials 15, no. 23: 8674. https://doi.org/10.3390/ma15238674

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop